HAYNES® 625SQ®

Principal Features

HAYNES® 625SQ® alloy (UNS N06626) is a solid-solution strengthened superalloy. It is a modification of HAYNES® 625 alloy developed to enhance resistance to fatigue at temperatures up to approximately 1200°F (649°C). The alloy composition is tightly controlled to very low levels of carbon, silicon, and nitrogen.

Primary melting is by vacuum induction melting, followed by consumable electrode practice using electroslag remelting. During processing, the grain size is controlled to ASTM #5 or finer.

HAYNES® 625SQ® alloy is readily fabricated and welded using practices common to HAYNES® 625 alloy. 625SQ® alloy sheet and strip find application in aerospace, automotive, and chemical process industry bellow, expansion joints, and fabrications where fatigue resistance, strength, and corrosion resistance are required.

*Please contact our technical support team if you have technical questions about this alloy.

Nominal Composition

Weight %
Nickel 62 Balance
Cobalt 1 max.
Iron 5 max.
Chromium 21
Molybdenum 9
Niobium* + Tantalum 3.7
Manganese 0.5 max.
Silicon 0.15 max.
Nitrogen 0.02 max.
Aluminum 0.4 max.
Titanium 0.4 max.
Carbon 0.03 max.

*Also known as Columbium

Physical Properties

Physical Property Customary Units Metric Units
Density RT
0.305lb/in3
RT
8.44 g/cm3
Melting Range 2350-2460°F – 1290-1350ºC –
Thermal Conductivity 800°F
109 Btu-in/ft2-hr-°F
1290-1350°C 15.3 W/m-°C
1000°F
121 Btu-in/ft2-hr-°F
400°C 18.3 W/m-°C
1200°F
132 Btu-in/ft2-hr-°F
600°C 19.8 W/m-°C
1400°F
144 Btu-in/ft2-hr-°F
700°C 21.5 W/m-°C
1600°F
158 Btu-in/ft2-hr-°F
800°C 23.4 W/m-°C
1800°F
175 Btu-in/ft2-hr-°F
900°C 25.6 W/m-°C
Mean Coefficient of Thermal Expansion 70-800°F 7.7 µin/in-°F 1000°C 14.2 µm/m-°C
70-1000°F 8.0 µin/in-°F 20-500°C 14.8 µm/m-°C
70-1200°F 8.2 µin/in-°F 20-600°C 15.4 µm/m-°C
70-1400°F 8.6 µin/in-°F 20-700°C 16.1 µm/m-°C
70-1600°F 9.2 µin/in-°F 20-800°C 16.8 µm/m-°C
70-1800°F 9.6 µin/in-°F 20-900°C 17.4 µm/m-°C
Electrical Resistivity 400°F 52.8 µohm-in 20-1000°C 134.0 µohm-cm
800°F 53.5 µohm-in 200°C 135.6 µohm-cm
1000°F 54.3 µohm-in 400°C 137.9 µohm-cm
1200°F 54.3 µohm-in 600°C 137.5 µohm-cm
1400°F 53.9 µohm-in 700°C 136.5 µohm-cm
1600°F 53.5 µohm-in 800°C 135.6 µohm-cm
1800°F 53.1 µohm-in 900°C 134.8 µohm-cm
Dynamic Modulus of Elasticity 70°F
30.2 x 106 psi
1000°C 208 GPa
400ºF
28.8 x 106 psi
20°C 199 GPa
800°F
26.7 x 106 psi
200°C 186 GPa
1000°F
25.6 x 106 psi
400°C 171 GPa
1200°F
24.3 x 106 psi
600°C 163 GPa
1400°F
22.8 x 106 psi
700°C 153 GPa
1600°F
21.2 x 106 psi
800°C 142 GPa
1800°F
18.7 x 106 psi
900°C 126 GPa

Tensile Properties

Sheet (AMS 5879)

Test Temperature Yield Strength 0.2% Offset Ultimate Tensile Strength Elongation
°F °C ksi MPa ksi MPa %
RT RT 65.5 452 129.9 895 51.7
600 316 51.1 353 117.4 809 64.1
800 427 49.1 339 112.6 776 60.9
1000 538 49.9 344 112.5 776 60.5
1200 649 46.9 323 114.2 787 81.4
1300 704 44.4 306 93.7 646 103.9
1400 760 46.9 323 72.1 497 88.8

RT= Room Temperature

Heat Treatment

Sheet and Strip, AMS 5879

1600 °F (871 °C) Minimum/Bright Anneal

Specifications and Codes

Specifications

HAYNES® 625SQ® alloy (N06626)
Sheet, Plate & Strip AMS 5879ASME CodeCase 2276
Billet, Rod & Bar –
Coated Electrodes –
Bare Welding Rods & Wire –
Seamless Pipe & Tube –
Welded Pipe & Tube ASME CodeCase No. 2276P= 43
Fittings ASME CodeCase No. 2276P= 43
Forgings –
DIN –
Others –

Codes

HAYNES® 625SQ® alloy (N06626)
ASME Section l –
Section lll Class 1 –
Class 2 –
Class 3 –
Section lV HF-300.2 –
Section Vlll Div. 1
Code Case 2276800°F (427°C)1
Div. 2 –
Section Xll –
B16.5 –
B16.34 –
B31.1 –
B31.3 –

Disclaimer

Haynes International makes all reasonable efforts to ensure the accuracy and correctness of the data displayed on this site but makes no representations or warranties as to the data’s accuracy, correctness or reliability. All data are for general information only and not for providing design advice. Alloy properties disclosed here are based on work conducted principally by Haynes International, Inc. and occasionally supplemented by information from the open literature and, as such, are indicative only of the results of such tests and should not be considered guaranteed maximums or minimums.  It is the responsibility of the user to test specific alloys under actual service conditions to determine their suitability for a particular purpose.

For specific concentrations of elements present in a particular product and a discussion of the potential health affects thereof, refer to the Safety Data Sheets supplied by Haynes International, Inc.  All trademarks are owned by Haynes International, Inc., unless otherwise indicated.

Alloy Brochure

Principal Features
Nominal Composition
Physical Properties
Tensile Properties
Heat Treatment
Specifications and Codes
Disclaimer
Alloy Brochure
Principal Features
Principal Features
Nominal Composition
Physical Properties
Tensile Properties
Heat Treatment
Specifications and Codes
Disclaimer
Alloy Brochure

Footer