HAYNES® 230®

Principal Features

HAYNES® 230® (UNS N06230) alloy is a nickel-chromium-tungsten-molybdenum alloy that combines excellent high-temperature strength, outstanding resistance to oxidizing environments up to 2100°F (1149°C) for prolonged exposures, premier resistance to nitriding environments, and excellent long-term thermal stability. It is readily fabricated and formed, and is castable. Other attractive features include lower thermal expansion characteristics than most high-temperature alloys, and a pronounced resistance to grain coarsening with prolonged exposure to high temperatures.

Easily Fabricated

HAYNES® 230® alloy has excellent forming and welding characteristics. It may be forged or otherwise hot-worked, providing it is held at 2150°F (1177°C) for a time sufficient to bring the entire piece to temperature. As a consequence of its good ductility, 230® alloy is also readily formed by cold-working. All hot- or cold-worked parts should be annealed and rapidly cooled in order to restore the best balance of properties. The alloy can be welded by a variety of techniques, including gas tungsten arc (GTAW), gas metal arc (GMAW), and resistance welding.

Heat Treatment

Wrought 230® alloy is furnished in the solution heat treated condition, unless otherwise specified. The alloy is solution heat-treated in the range of 2150 to 2275°F (1177 to 1246°C) and rapidly cooled or water-quenched for optimum properties.

Annealing at temperatures lower than the solution heat treating temperatures will produce some carbide precipitation in 230® alloy, which may marginally affect the alloy’s strength and ductility.

Applications

HAYNES® 230® alloy combines properties which make it ideally suited for a wide variety of component applications in the aerospace and power industries. It is used for combustion cans, transition ducts, flame holders, thermocouple sheaths, and other important gas turbine components. In the chemical process industry, 230® alloy is used for catalyst grid supports in ammonia burners, high-strength thermocouple protection tubes, high-temperature heat exchangers, ducts, high-temperature bellows, and various other key process internals.

In the industrial heating industry, applications for 230 alloy include furnace retorts, chains and fixtures, burner flame shrouds, recuperator internals, dampers, nitriding furnace internals, heat-treating baskets, grates, trays, sparger tubes, thermocouple protection tubes, cyclone internals, and many more.

*Please contact our technical support team if you have technical questions about this alloy.

Nominal Composition

Weight %
Nickel 57 Balance
Chromium 22
Tungsten 14
Molybdenum 2
Iron 3 max.
Cobalt 5 max.
Manganese 0.5
Silicon 0.4
Niobium 0.5 max.
Aluminum 0.3
Titanium 0.1 max.
Carbon 0.1
Lanthanum 0.02
Boron 0.015 max.

Creep and Stress-rupture Strength

HAYNES® 230® alloy is a solid-solution-strengthened material which combines excellent high-temperature strength with good fabricability at room temperature. It is particularly effective for very long-term applications at temperatures of 1200°F (650°C) or more, and is capable of outlasting stainless steels and nickel alloys by as much as 100 to 1 depending upon the temperature. Alternatively, the higher strength of 230® alloy allows for the use of design section thicknesses as much as 75 percent thinner than lesser alloys with no loss in load-bearing capability.

Stress-Rupture Lives for Various Alloys at Fixed Test Conditions (Bar and Plate)*

Alloy Hours to Rupture
1400°F (760°C) 1600°F (871°C) 1800°F (982°C)
– 15.0 ksi (103 MPa) 4.1 ksi (31 Mpa) 2.0 ksi (14 Mpa)
230® 8,200 65,000 5,000
625 19,000 14,000 2,400
X 900 5,000 2,100
800H 130 1,200 920
INCONEL® 601 50 1,200 1,000
253 MA® 140 900 720
600 15 280 580
316 SS 100 240 130
RA330® 30 230 130
304 SS 10 100 72

*Based upon Larson-Miller extrapolation

Comparison of Stress to Produce 1% Creep in 1000 Hours (Sheet)

230® Sheet, Solution Annealed

Temperature Creep Approximate Initial Stress to Produce Specified Creep in
10 Hours 100 Hours 1,000 Hours 10,000 Hours
°F °C % ksi MPa ksi MPa ksi MPa ksi MPa
1200 649 0.5 – – 31 214 – – – —
1 – – 35 241 24* 165* – —
R – – 51 352 36 248 28 193
1300† 704 0.5 29 200 21 145 15 100 – —
1 33 228 23 159 17 114 – —
R 47 324 34 234 26 179 20 134
1400 760 0.5 19 132 14 94 9.6 66 7.3 50
1 21 145 16 107 12 79 8.6 59
R 32 221 25 169 18 125 13* 91*
1500 816 0.5 14 98 10 71 7.5 52 5.4* 37*
1 15 103 11 77 8.6 59 6.5* 45*
R 23* 161* 18 121 13 86 8.4* 58*
1600 871 0.5 11 78 8.1 56 5.7 39 4.0 28
1 12 81 9.0 62 6.2 43 4.3 30
R 17 117 12.5 86 8.2 57 5.6* 39*
1700 927 0.5 7.7 53 5.5 38 3.8 26 2.4* 17*
1 8.8* 61* 6.2 43 4.2 29 2.7* 19*
R 12.0* 83* 8.0 55 5.1 35 3.2 22
1800 982 0.5 7.0 48 3.6 25 1.8 12 0.85 5.9
1 8.0 55 4.1 28 2.0 14 1.0 6.9
R 10.0 69 5.4 37 2.6 18 1.2* 8.3*
1900 1038 0.5 – – 1.7 12 0.8 5.5 – —
1 – – 2.0 14 0.9 6.2 – —
R – – 3.0* 21* 1.5 10 – —
2000 1093 0.5 – – – – – – – —
1 – – 0.9 6.2 – – – —
R – – – – – – – —

*Significant extrapolation
† Values obtained using Larson-Miller interpolation

230® Plate, Solution Annealed

Temperature Creep Approximate Initial Stress to Produce Specified Creep in
10 Hours 100 Hours 1,000 Hours 10,000 Hours
°F °C % ksi MPa ksi MPa ksi MPa ksi MPa
1200 649 0.5 – – 35 241 23 159 – –
1 – – 39 269 26.5 183 17.5 121
R 75 517 56 386 41 283 29 200
1300 704 0.5 35 241 21.5 148 14.5 100 – –
1 39 269 24.5 169 18 124 12.3* 85*
R 59 407 42 290 30 207 21 145
1400 760 0.5 19 131 13.5 93 10.0 69 – –
1 23 159 15.9 110 11.5 79 9.0* 62*
R 37 255 27 186 20 138 14.2 98
1500 816 0.5 14.0 97 10.4 72 8.2 57 6.1 42
1 16.5 114 12.5 86 9.5 66 6.9 48
R 26 179 20 138 14.0 97 9.8 68
1600 871 0.5 10.3 71 7.6 52 5.6 39 4.0 28
1 11.7 81 9.0 62 6.2 43 4.3 30
R 20 138 13.7 94 9.5 66 6.2 43
1700 927 0.5 7.8 54 5.7 39 3.9 27 2.5 17
1 8.8 61 6.8 47 4.5 31 2.7 19
R 15.0 103 10.0 69 6.0 41 3.6 25
1800 982 0.5 5.8 40 3.5 24 1.8 12 0.90 6.2
1 6.3 43 4.0 28 2.1 14 1.1 7.6
R 9.4 65 6.0 41 3.2 22 1.7 12
1900 1038 0.5 4.0 28 2.0 14 0.90 6.2 – –
1 4.4 30 2.2 15 1.0 6.9 0.50* 3.4*
R 7.0 48 3.7 26 1.8 12 1.0 6.9
2000 1093 0.5 1.9 13 0.80 5.5 0.35 2.4 – –
1 2.3 16 1.0 6.9 0.47 3.2 0.20* 1.4*
R 4.2 29 2.1 14 1.0 6.9 0.55 3.8
2100 1149 0.5 0.80 5.5 0.03* 2.1* – – – –
1 1.0 6.9 0.43 3.0 – – – –
R 2.3 16 1.2 8.3 0.60 4.1 – –

*Significant extrapolation

Low Cycle Fatigue

HAYNES® 230® alloy exhibits excellent low cycle fatigue properties at elevated temperature. Results shown below are for strain-controlled tests run in the temperature range from 800 to 1800°F (425 to 980°C). Samples were machined from plate. Tests were run with fully reversed strain (R=-1) at a frequency of 20 cpm (0.33 Hz).

Comparative Low Cycle Fatigue Properties

The graph below compares the low cycle fatigue lives of a number of alloys tested at 800°F (427°C) in both the as-received and 1400°F (760°C)/1000 hour pre-exposed condition. Samples were machined from plate or bar, after exposure for exposed samples. Tests were again run with fully reversed strain (R=-1) at a frequency of 20 cpm (0.33 Hz). TSR=Total Strain Range.

800°F (425°C) LCF Life for Various Alloys

Compilation of axial LCF test results (R=-1, f=0.33 Hz)

Temperature
Δεtot/%
Ni, Cycles to Initiation
Nf, Cycles to Failure
°F °C - - -
800 427 1.50 2230 2398
1.00 8480 8742
0.80 14,918 16,575
0.65 45,127 46,523
0.55 103,910 115,456
1000 538 1.50 1329 1540
1.25 1974 2368
1.00 3330 4413
0.80 7864 8734
0.70 8423 9876
0.60 38,696 40,604
0.56 73,014 74,132
0.53 -- 200,005*
0.50 -- 201,190*
1200 649 1.25 1022 1257
1.00 1852 2254
0.80 3431 4248
0.60 8962 11,058
0.50 82,275 85,563
0.45 -- 200,002*
0.40 -- 200,005*
1400 760 0.80 1896 2218
0.40 20,519 21,564
0.40 43,915 45,279
0.30 -- 203,327*
1400 760 1.00 870 1097
1.00 827 990
0.70 3166 3622
0.50 8153 8490
0.40 51,285 57,819
0.40 68,451 75,470
0.38 95,165 96,844
0.37 91,879 97,612
0.35 -- 202,920*
0.30 -- 150,000*
1600 871 0.70 1279 1504
0.50 3939 4299
0.50 3176 3473
0.40 9712 10,837
0.40 9296 10,781
0.35 19,179 20,964
0.31 61,898 63,253
0.30 65,691 66,926
0.25 -- 200,770*
1800 982 0.60 818 1218
0.50 1506 2582
0.40 3520 4223
0.40 3070 4784
0.30 19,810 21,311
0.30 13,904 19,200
0.25 105,140 106,020
0.25 116,960 119,890

* Indicates a run-out.

Tensile Properties

Tensile Properties of 230® Sheet

Test Temperature 0.2% Yield Strength Ultimate Tensile Strength Elongation
°F °C ksi MPa ksi MPa %
70 21 60.4 417 121.4  837 47.3
1000 538 42.6 294 100.1 690 51.7
1200 649 42.2 291 96.6 666 56.9
1400 760 45.1 311 78.0 538 59.5
1600 871 34.2 236 44.6 308 74.2
1800 982 17.8 123 24.5 169 54.1
2000 1093 10.0 69 13.1 90 37.0

Tensile Properties of 230® Plate

Test Temperature 0.2% Yield Strength Ultimate Tensile Strength Elongation
°F °C ksi MPa ksi MPa %
70 21 55.5 383 123.6 852 46.0
1000 538 38.1 263 102.5 706 53.2
1200 649 38.7 267 98.2 677 53.0
1400 760 37.7 260 77.2 533 68.0
1600 871 33.9 234 45.1 311 94.0
1800 982 16.8 116 24.3 168 91.2
2000 1093 9.1 63 13.2 91 92.1

Comparison of Yield Strengths (Plate)

Thermal Stability

HAYNES® 230® alloy exhibits excellent retained ductility after long-term thermal exposure at intermediate temperatures. It does not exhibit sigma phase, mu phase, or other deleterious phase formation even after 16,000 hours of exposure at temperatures from 1200 to 1600°F (649 to 871°C). Principal phases precipitated from solid solution are all carbides.

This contrasts markedly with many other solid-solution-strengthened superalloys such as HAYNES® 188 alloy, HAYNES® 625 alloy, and HASTELLOY® X alloy. These alloys all precipitate deleterious phases, which impair both tensile ductility and impact strength.

other solid-solution-strengthened superalloys such as HAYNES® 188 alloy, HAYNES® 625 alloy, and HASTELLOY® X alloy. These alloys all precipitate deleterious phases, which impair both tensile ductility and impact strength.

Room-Temperature Properties after Thermal Exposure

Condition 0.2% Yield Strength Ultimate Tensile Strength Elongation R.A. Impact Strength
- ksi ksi % % ft-lb
MA 58.4 123.1 50 47.2 54
+ 1200/8,000 hr 57.9 128.0 36.4 39 31.4
+ 1200/20,000 hr 57.6 128.4 34.8 37 28.9
+ 1200/30,000 hr 59.4 129.9 34 38.3 –
+ 1200/50,000 hr 61.2 131.7 33.9 36.9 25.8
+1400/8,000 hr 59.2 129.7 32 34.3 18.7
+1400/20,000 hr 55 126.9 31.2 31.6 18.8
+1400/30,000 hr 54.3 126.9 31.3 33.9 –
+1400/50,000 hr 55.2 127.7 32.2 32.5 20.7
+ 1600/8,000 hr 54.3 122.7 36.2 34.6 21.6
+ 1600/20,000 hr 50.1 121.6 34.4 31.1 19.5
+ 1600/30,000 hr 49.6 120.0 32.1 28.6 –
+ 1600/50,000 hr 50.4 116.7 25.2* 20.2 14.8

*BIGM; AGL Elong, which tends to be lower; Other data are 4D Elong.
R.A.= Reduction of Area

Retained Room Temperature Tensile Ductility after 8000 Hour Exposure at Temperature

Exposure Temperature 230® 188 625 X
Room Temperature Tensile Elongation
°F % % % %
1200 36.4 29.1 18 19
1400 32 10.8 13 19
1600 36.2 22.2 26 30

Resistance to Grain Growth

HAYNES® 230® alloy exhibits excellent resistance to grain growth at high temperatures. As a consequence of its very stable primary carbides, 230® alloy can be exposed at temperatures as high as 2200°F (1204°C) for up to 24 hours without exhibiting significant grain growth. Materials such as HAYNES® 188 alloy or HASTELLOY® X alloy exhibit greater grain growth under such conditions, as would most iron-, nickel-, or cobalt-base alloys and stainless steels.

Exposure Time Grain Size for Alloys Exposed at Temperature for Various Times*
HAYNES® 230® alloy HAYNES® 188 alloy HASTELLOY® X alloy
h 2150°F (1177°C)  2200°F (1204°C)  2150°F (1177°C) 2200°F (1204°C)  2150°F (1177°C) 2200°F (1204°C) 
0 4-4 1/2 4-4 1/2 4-5 4-5 3 1/2 3 1/2
1 4-5 4-4 1/2 2-5 2-4 3 1/2 0-1
4 4-4 1/2 4-4 1/2 3 1/2 3 3 1/2 0-1
24 4 4-4 1/2 0-2 1-3 00-4 0-1 1/2

*Plate Product in the fully annealed condition

Physical Properties

Physical Property Customary Units Metric Units
Density RT
0.324 lb/in3
RT
8.97 g/cm3
Melting Temperature 2400 - 2570°F – 1301 - 1371°C –
Electrical Resistivity RT 49.2 µohm-in RT 125.0 µohm-cm
200°F 49.5 µohm-in 100°C 125.8 µohm-cm
400°F 49.8 µohm-in 200°C 126.5 µohm-cm
600°F 50.2 µohm-in 300°C 127.3 µohm-cm
800°F 50.7 µohm-in 400°C 128.4 µohm-cm
1000°F 51.5 µohm-in 500°C 130.2 µohm-cm
1200°F 51.6 µohm-in 600°C 131.2 µohm-cm
1400°F 51.1 µohm-in 700°C 130.7 µohm-cm
1600°F 50.3 µohm-in 800°C 129.1 µohm-cm
1800°F 49.3 µohm-in 900°C 127.1 µohm-cm
- - 1000°C 125.0 µohm-cm
Thermal Diffusivity RT
3.8 x 10-3 in2/sec
RT
24.2 x 10-3 cm2/s
200°F
4.1 x 10-3 in2/sec
100°C
26.8 x 10-3 cm2/s
400°F
4.7 x 10-3 in2/sec
200°C
29.9 x 10-3 cm2/s
600°F
5.2 x 10-3 in2/sec
300°C
32.9 x 10-3 cm2/s
800°F
5.6 x 10-3 in2/sec
400°C
35.7 x 10-3 cm2/s
1000°F
6.1 x 10-3 in2/sec
500°C
38.5 x 10-3 cm2/s
1200°F
6.5 x 10-3 in2/sec
600°C
41.9 x 10-3 cm2/s
1400°F
6.7 x 10-3 in2/sec
700°C
43.0 x 10-3 cm2/s
1600°F
6.7 x 10-3 in2/sec
800°C
43.2 x 10-3 cm2/s
1800°F
7.3 x 10-3 in2/sec
900°C
44.4 x 10-3 cm2/s
- - 1000°C
48.2 x 10-3 cm2/s
Thermal Conductivity RT
62 Btu-in/ft2-hr-°F
RT 8.9 W/m-°C
200°F
71 Btu-in/ft2-hr-°F
100°C 10.4 W/m-°C
400°F
87 Btu-in/ft2-hr-°F
200°C 12.4 W/m-°C
600°F
102 Btu-in/ft2-hr-°F
300°C 14.4 W/m-°C
800°F
118 Btu-in/ft2-hr-°F
400°C 16.4 W/m-°C
1000°F
133 Btu-in/ft2-hr-°F
500°C 18.4 W/m-°C
1200°F
148 Btu-in/ft2-hr-°F
600°C 20.4 W/m-°C
1400°F
164 Btu-in/ft2-hr-°F
700°C 22.4 W/m-°C
1600°F
179 Btu-in/ft2-hr-°F
800°C 24.4 W/m-°C
1800°F
195 Btu-in/ft2-hr-°F
900°C 26.4 W/m-°C
- - 1000°C 28.4 W/m-°C
Specific Heat RT 0.095 Btu/lb-°F RT 397 J/kg·°C
200°F 0.099 Btu/lb-°F 100°C 419 J/kg·°C
400°F 0.104 Btu/lb-°F 200°C 435 J/kg·°C
600°F 0.108 Btu/lb-°F 300°C 448 J/kg·°C
800°F 0.112 Btu/lb-°F 400°C 465 J/kg·°C
1000°F 0.112 Btu/lb-°F 500°C 473 J/kg·°C
1200°F 0.134 Btu/lb-°F 600°C 486 J/kg·°C
1400°F 0.140 Btu/lb-°F 700°C 574 J/kg·°C
1600°F 0.145 Btu/lb-°F 800°C 595 J/kg·°C
1800°F 0.147 Btu/lb-°F 900°C 609 J/kg·°C
- - 1000°C 617 J/kg·°C
Mean Coefficient of Thermal Expansion 70 - 200°F 6.5 µin/in -°F 25 - 100°C
11.8 x 10-6 m/m·°C
70 - 400°F 6.9 µin/in -°F 25 - 200°C
12.4 x 10-6 m/m·°C
70 - 600°F 7.2 µin/in -°F 25 - 300°C
12.8 x 10-6 m/m·°C
70 - 800°F 7.4 µin/in -°F 25 - 400°C
13.2 x 10-6 m/m·°C
70 - 1000°F 7.6 µin/in -°F 25 - 500°C
13.6 x 10-6 m/m·°C
70 - 1200°F 8.0 µin/in -°F 25 - 600°C
14.1 x 10-6 m/m·°C
70 - 1400°F 8.3 µin/in -°F 25 - 700°C
14.7 x 10-6 m/m·°C
70 - 1600°F 8.6 µin/in -°F 25 - 800°C
15.2 x 10-6 m/m·°C
70 - 1800°F 8.9 µin/in -°F 25 - 900°C
15.7 x 10-6 m/m·°C
- - 25 - 1000°C
16.1 x 10-6 m/m·°C
Dynamic Modulus of Elasticity RT
30.3 x 106 psi
RT 209 GPa
200°F
30.1 x 106 psi
100°C 207 GPa
400°F
29.0 x 106 psi
200°C 200 GPa
600°F
27.8 x 106 psi
300°C 193 GPa
800°F
26.8 x 106 psi
400°C 186 GPa
1000°F
25.9 x 106 psi
500°C 181 GPa
1200°F
24.9 x 106 psi
600°C 175 GPa
1400°F
23.6 x 106 psi
700°C 168 GPa
1600°F
22.2 x 106 psi
800°C 159 GPa
1800°F
20.7 x 106 psi
900°C 150 GPa
2000ºF
19.1 x 106 psi
1000°C 141 GPa
Dynamic Shear Modulus RT
11.5 106 psi
RT 79 GPa
200°F
11.4 106 psi
100°C 79 GPa
400°F
11.0 106 psi
200°C 76 Gpa
600°F
10.5 x 106 psi
300°C 73 GPa
800°F
10.1 x 106 psi
400°C 70 GPa
1000°F
9.7 x 106 psi
500°C 67 GPa
1200°F
9.3 x 106 psi
600°C 64 GPa
1400°F
8.8 x 106 psi
700°C 61 GPa
1600°F
8.2 x 106 psi
800°C 57 GPa
1800°F
7.6 x 106 psi
900°C 52 GPa
2000°F
7.0 x 106 psi
1000°C 48 GPa
Poisson’s Ratio RT 0.31 RT 0.31
200°F 0.31 100°C 0.31
400°F 0.32 200°C 0.32
600°F 0.32 300°C 0.32
800°F 0.33 400°C 0.33
1000°F 0.33 500°C 0.33
1200°F 0.34 600°C 0.34
1400°F 0.34 700°C 0.34
1600°F 0.35 800°C 0.34
1800°F 0.36 900°C 0.35

*RT= Room Temperature

Thermal Expansion Characteristics

HAYNES® 230® alloy has relatively low thermal expansion characteristics compared to most high-strength superalloys, iron-nickel-chromium alloys, and austenitic stainless steels. This means lower thermal stresses in service for complex component fabrications, as well as tighter control over critical part dimensions and clearances.

Oxidation Resistance

HAYNES® 230® alloy exhibits excellent resistance to both air and combustion gas oxidizing environments, and can be used for long-term continuous exposure at temperatures up to 2100°F (1150°C). For exposures of short duration, 230® alloy can be used at higher temperatures.

Schematic Representation of Metallographic Technique used for
Evaluating Oxidation Tests

Comparative Dynamic Oxidation

Alloy 1600°F (870°C), 2000 h, 30-min cycles 1800°F (980°C), 1000 h, 30-min cycles 2000°F (1090°C), 500 h, 30-min cycles 2100°F (1150°C), 200 h, 30-min cycles
Metal Loss Average Metal Affected Metal Loss Average Metal Affected Metal Loss Average Metal Affected Metal Loss Average Metal Affected
- mils µm mils µm mils µm mils µm mils µm mils µm mils µm mils µm
188 1.1 28 2.9 74 1.1 28 3.2 81 10.9 277 13.1 333 8 203 9.7 246
230® 0.9 23 3.9 99 2.8 71 5.6 142 7.1 180 9.9 251 6.4 163 13.1 333
617 2 51 7.8 198 2.4 61 5.7 145 13.3 338 20.9 531 13.8 351 15.3 389
625 1.2 30 2.2 56 3.7 94 6 152 – – Consumed – – – –
556® 1.5 38 3.9 99 4.1 104 6.7 170 9.9 251 12.1 307 11.5 292 14 356
X 1.7 43 5.3 135 4.3 109 7.3 185 11.6 295 14 356 13.9 353 15.9 404
HR-120® – – – – 6.3 160 8.3 211 – – – – – – – –
RA330 2.5 64 5 127 8.7 221 10.5 267 15.4 391 17.9 455 11.5 292 13 330
HR-160® – – – – 5.4 137 11.9 302 12.5 18.1 460 8.7 221 15.5 394
310SS 6 152 7.9 201 16 406 18.3 465 – – – – – – Consumed
800H 3.9 99 9.4 239 22.9 582 Through Thickness – – Consumed after 300 h – – Consumed

Burner rig oxidation tests were conducted by exposing samples of 3/8” x 2.5” x thickness (9mm x 64 mm x thickness), in a rotating holder to the products of combustion of 2 parts No. 1 and 1 part No. 2 fuel burned at a ratio of air to fuel of about 50:1. Gas velocity was about 0.3 mach. Samples were automatically removed from the gas stream every 30 minutes and fan-cooled to near ambient temperature and then reinserted into the flame tunnel.

Comparative Oxidation in Flowing Air 2100°F (1150°C) for 1008 Hours

Microstructures shown are for coupons exposed for 1008 hours at 2100°F (1150°C) in air flowing 7.0 feet/minute (2.1 m/minute) past the samples. Samples were descaled by cathodically charging the coupons while they were immersed in a molten salt solution. The black area shown at the top of each picture represents actual metal loss due to oxidation. The data clearly show HAYNES® 230® alloy to be superior to both INCONEL alloy 601 and alloy 800H, as well as the other heat-resistant materials listed in the table above.

230® alloy
Average Metal Affected
= 3.4 mils (86 µm)

INCONEL alloy 601
Average Metal Affected
= 5.3 mils (135 µm)

Alloy 800H
Average Metal Affected
= 8.9 mils (226 µm)

Water Vapor Testing

Alloy
1008 hours @ 1600F Cycled 1x/week in air+10%H2O
1008 hours @ 1600F Cycled 1x/week in air+20%H2O
6 months @ 1400F Cycled 1x/week in air+10%H2O
Metal Loss Average Metal Affected Metal Loss Average Metal Affected Metal Loss Average Metal Affected
- mils per side mm per side mils per side mm per side mils per side mm per side mils per side mm per side mils per side mm per side mils per side mm per side
230® 0.07 0.002 0.53 0.013 0.03 0.001 0.21 0.005 0.05 0.001 0.35 0.009
625 0.11 0.003 0.5 0.013 0.04 0.001 0.27 0.007 - - - -
X 0.03 0.001 0.5 0.013 0.04 0.001 0.3 0.008 - - - -
253MA 0.66 0.017 1.59 0.040 0.08 0.002 0.68 0.017 - - - -
800HT - - - - - - - - 0.12 0.003 0.82 0.021
347SS 0.86 0.022 1.48 0.038 0.18 0.005 0.18 0.005 0.46 0.012 1.26 0.032

Amount of metal affected for high‐temperature sheet (0.060 ‐ 0.125”) alloys exposed for 360 days (8,640 h) in flowing air.

Alloy 1600°F 1800°F 2000°F 2100°F
Metal Loss* Average Metal Affected Metal Loss* Average Metal Affected Metal Loss* Average Metal Affected Metal Loss* Average Metal Affected
- mils µm mils µm mils µm mils µm mils µm mils µm mils µm mils µm
625 0.3 8 1.4 36 – – – – – – – – – – – –
230® 0.2 5 1.4 36 0.1 3 2.5 64 3.4 86 11 279 28.5 724 34.4 874
617 0.3 8 1.6 41 – – – – – – – – – – – –
HR‐120® 0.3 8 1.6 41 0.5 13 3.3 84 18.1 460 23.2 589 33.6 853 44 1118
25 0.3 8 1.7 43 – – – – – – – – – – – –
188 0.2 5 1.8 46 – – – – – – – – – – – –
556® 0.3 8 1.9 48 0.5 13 6.2 157 15 381 24.1 612 – – – –
X 0.3 8 2.2 56 0.2 5 2.8 71 17.1 434 26.2 665 51.5 1308 55.4 1407
800HT 0.4 10 2.9 74 – – – – – – – – – – – –
HR-160® – – – – 1.7 43 13.7 348 7.2 183 30.8 782 12 305 45.6 1158

*Metal loss was calculated from final and initial metal thicknesses; i.e. ML = (OMT – FMT) /2

Static Oxidation Comparison

Scroll for more Data

Alloy Comparative Oxidation Resistance in Flowing Air, 1008 Hours*
1800°F (982°C) 2000°F (1093°C) 2100°F (1149°C) 2200°F (1204°C)
Metal Loss* Average Metal Affected Metal Loss* Average Metal Affected Metal Loss* Average Metal Affected Metal Loss* Average Metal Affected
- mils µm mils µm mils µm mils µm mils µm mils µm mils µm mils µm
230® 0.2 5 1.5 38 0.5 13 3.3 84 1.2 30 4.4 112 4.7 119 8.3 211
188 0.1 3 1.1 28 0.5 13 3.7 94 8.6 218 10.7 272 5.2 132 48.2 1224
601 0.4 10 1.7 43 1.3 33 3.8 97 2.8 71 6.5 165 4.4 112 7.5 191
617 0.3 8 2 51 0.6 15 3.8 97 1 25 5.2 132 10.7 272 12.6 320
X 0.2 5 1.5 38 1.3 33 4.4 112 3.6 91 6.1 115 – – – –
800HT 0.5 13 4.1 104 7.6 193 11.6 295 12.4 315 15 381 – – – –
446 SS – – – – 13 330 14.4 366 – – >21.5 >546 – – – –
316 SS 12.3 312 14.2 361 – – >17.5 >445 – – >17.5 >445 – – – –

*Metal Loss + Average Internal Penetration.

Nitriding Resistance

HAYNES® 230® alloy is one of the most nitriding resistant materials commercially available. Tests were performed in flowing ammonia at 1200°F (650°C) and 1800°F (980°C) for 168 hours. Nitrogen absorption was determined by chemical analysis of samples before and after exposure and knowledge of the exposed specimen area.

Alloy
Nitrogen Absorption (mg/cm2)
- 1200°F (649°C) 1800°F (982°C) 2000°F (1093°C)
230® 0.7 1.4 1.5
600 0.8 0.9 0.3
625 0.8 2.5 3.3
X 1.7 3.2 3.8
RA330® – 3.9 3.1
800H 4.3 4.0 5.5
316 SS 6.9 6.0 3.3
310 SS 7.4 7.7 9.5
304 SS 9.8 7.3 3.5

Carburization Resistance

HAYNES® 230® alloy exhibits good resistance to carburization when compared with many other industrial alloys. Test results were generated for 500 hours exposure in packed graphite at 1800°F (980°C). Carbon absorption was determined by chemical analysis of samples before and after exposure and knowledge of the exposed specimen area.

Hydrogen Embrittlement

Notched tensile tests performed in hydrogen and air reveal that 230® alloy is resistant to hydrogen embrittlement. Tests were performed in MIL-P-27201B grade hydrogen, with a crosshead speed of 0.005 in/min (0.13 mm/min). Specimens were notched with a KT value of 8.0.

Test Temperature Hydrogen Pressure Ratio of Notched Tensile Strength, Hydrogen/Air
°F °C psi MPa –
70 21 3000 21 0.92
70 21 5000 34 1.07

Aqueous Corrosion Resistance

Coupons were exposed for four 24-hour periods in various acids at the stated temperatures, and general corrosion rates were calculated from weight change measurements.

Alloy Corrosion Rate (mils per year)
–
10% HNO3 Boiling
10% H2SO4 150°F (66°C)
10% HCl 150°F (66°C)
230® 0.3 0.6 112
625 0.7 0.4 65
600 0.8 41.8 366
316 SS 1.0 17.8 3408
X – <0.1 99

Hardness and Grain Size

Solution Annealed Room Temperature Hardness

Form Hardness, HRBW Typical ASTM Grain Size
Sheet 92 4 – 6.5
Plate 92 3 – 5
Bar 90 3 – 5

HRBW = Hardness Rockwell “B”, Tungsten Indentor.

Applications

Nitric acid catalyst grids support made from HAYNES® 230® alloy plate and bar. Excellent creep strength at 1700°F (927°C) makes the alloy highly suitable for this application.
Textron Lycoming gas turbine engine combustor made of HAYNES® 230® alloy.
Prototype 230® combustor for Dresser-Rand DR-990 industrial turbine.
Prototype 230® high-temperature expansion bellows made of 0.020-inch (0.5mm) thick sheet in a catalytic cracker configuration.
This horizontal electrically fired 230® retort replaced an alloy 600 retort which lasted only an average of  eight months in 1400 to 2200°F (760 to 1205°C) service in hydrogen atmosphere.  The 230 retort was still in excellent condition after 24 months service, as shown.
Resistance-heated 230® superheater tubes at the Penn State Applied Research Laboratory.  Used to produce about 1625°F (885°C) high-pressure steam.
Wire annealing fixture of 230® alloy reduces thermal mass and cycle times after replacing massive carbon-steel «stub» used previously.
Fabricated heat-treating basket for vacuum furnace application to 2300°F (1260°C). Made from 1/2-inch (12.7 mm) diameter 230® bar.
This striking shot of a HAYNES® 230® heat-treat fixture was taken at a leading off-road automotive equipment plant.  This conveyor fixture operates at 1550°F (845°C) with a subsequent water quench followed by a four hour cycle at 1050°F (565°C).
HAYNES® 230® damper atop this glass melting furnace withstands 2300°F (1260°C) for short times and 2000°F (1095°C) for sustained periods.
Cast heat-treat basket of 230® alloy in use at Alloy Foundries, Division of the Eastern Company, Naugatuck, Connecticut.
Substrate holder and box  of 230® alloy resist temperatures of 1650°F (900°C) during the production of semiconductors.
230® retorts operate at 2100°F (1150°C) with a hydrogen atmosphere (inside) and combustion products outside.

Microstructure

Etchant 95ml
HCl plus 5 gm
oxalic acid, 4 volts

Welding

HAYNES® 230® alloy is readily welded by Gas Tungsten Arc Welding (GTAW), Gas Metal Arc Welding (GMAW), Shielded Metal Arc Welding (SMAW), and resistance welding techniques. Its welding characteristics are similar to those for HASTELLOY® X alloy. Submerged Arc Welding (SAW) is not recommended as this process is characterized by high heat input to the base metal and slow cooling of the weld.  These factors can increase weld restraint and promote cracking.

Base Metal Preparation

The welding surface and adjacent regions should be thoroughly cleaned with an appropriate solvent prior to any welding operation.   All greases, oils, cutting oils, crayon marks, machining solutions, corrosion products, paint, scale, dye penetrant solutions, and other foreign matter should be completely removed.  It is preferable, but not necessary, that the alloy be in the solution- annealed condition when welded.

Filler Metal Selection

HAYNES® 230-W® filler wire (AWS A5.14, ERNiCrWMo-1) is recommended for joining 230® alloy by Gas Tungsten Arc or Gas Metal Arc welding.  Coated electrodes of 230-W alloy are also available for Shielded Metal Arc welding.  For dissimilar metal joining of 230®  alloy to nickel-, cobalt-, or iron- base materials, 230-W®  filler wire, HAYNES® 556® alloy (AWS A5.9 ER3556, AMS 5831), HASTELLOY® S alloy (AMS 5838) or HASTELLOY® W alloy (AMS 5786, 5787) welding products may all be considered, depending upon the particular case. Please click here or the Haynes Welding SmartGuide for more information.

Preheating, Interpass Temperatures, and Postweld Heat Treatment

Preheat is not required. Preheat is generally specified as room temperature (typical shop conditions).   Interpass temperature should be maintained below 200°F (93°C). Auxiliary cooling methods may be used between weld passes, as needed, providing that such methods do not introduce contaminants.  Postweld heat treatment is not generally required for 230 alloy.  For further information, please click here.

Nominal Welding Parameters

Details for GTAW, GMAW and SMAW welding are given here. Nominal welding parameters are provided as a guide for performing typical operations and are based upon welding conditions used in our laboratories.

Room Temperature Transverse Weld Tensile Results – GTAW of 0.205-in / 5.2 mm Plate

0.2% Yield Strength Ultimate Tensile Strength Elongation Fracture Location
ksi MPa ksi MPa % -
60.2 415 117.7 812 29.6 Weld Metal
58.4 403 113.4 782 28.2 Weld Metal

Transverse Weld Tensile Results – GTAW of 0.5-in / 12.7 mm Plate

Temperature 0.2% Yield Strength Ultimate Tensile Strength Elongation Fracture Location
°F °C ksi MPa ksi MPa % -
Room Temperature 65.5 452 126.8 874 37.3 Weld Metal
63.8 440 120 827 27 Weld Metal
1600 871 38.4 265 60.6 418 44.9 Base Metal
34.8 240 61.8 426 28.9 Weld Metal

Room Temperature Transverse Weld Tensile Results – GMAW of 2.0-in / 50.8 mm Plate

Ultimate Tensile Strength Fracture Location
ksi MPa -
116 800 Weld Metal
117 807 Weld Metal
115 793 Weld Metal
116 800 Weld Metal

Room Temperature Transverse Weld Tensile Results – GTAW of 3.0-in / 76.2 mm Plate

Sample Location 0.2% Yield Strength Ultimate Tensile Strength Elongation Reduction of Area Fracture Location
- ksi MPa ksi MPa % % -
Weld Face 74.1 511 109.5 755 27.2 30.9 Weld Metal
74.6 514 110.7 763 34.8 44.4 Weld Metal
Weld Center 76.5 527 113.3 781 33.1 37.6 Weld Metal
76.8 530 111.2 767 26.7 32.9 Weld Metal
Weld Root 74.8 516 109.9 758 19.6 24.1 Weld Metal
74 510 115 793 31 41.3 Weld Metal

HAYNES® 230-W® All-Weld-Metal Tensile Test Results

Test Temperature 0.2% Yield Strength Ultimate Tensile Strength Elongation
°F °C ksi MPa ksi MPa %
RT RT 75.7 520 112.6 775 27.3
1800 980 21.2 145 22.7 155 24.6

Specifications and Codes

Specifications

HAYNES® 230® alloy (N06230)
Sheet, Plate & Strip AMS 5878 SB 435/B 435 P= 43
Billet, Rod & Bar AMS 5891 SB 572/B 572 B 472 P= 43
Coated Electrodes SFA 5.11/ A 5.11 (ENiCrWMo-1) F= 43
Bare Welding Rods & Wire SFA 5.14/ A 5.14 (ERNiCrWMo-1) AMS 5839 F= 43
Seamless Pipe & Tube SB 622/B 622 P= 43
Welded Pipe & Tube SB 619/B 619 SB 626/B 626 P= 43
Fittings SB 366/B 366 P= 43
Forgings AMS 589 1SB 564/B 564 P= 43
DIN 17744 No. 2.4733 NiCr22W14Mo
Others –

Codes

HAYNES® 230® alloy (N06230)
ASME Section l

1650°F (899°C)1

Section lll Class 1 –
Class 2 –
Class 3 –
Section lV HF-300.2

500°F (132°C)1

Section Vlll Div. 1

1800°F (982°C)1

Div. 2 –
Section Xll

650°F (343°C)1

B16.5

1500°F (816°C)11

B16.34

1500°F (816°C)6

B31.1 –
B31.3

1650°F (900°C)1

MMPDS 6.3.9

1Plate, Sheet, Bar, Forgings, fittings, welded pipe/tube, seamless pipe/tube
2Plate, Forgings
3Plate, Bar, Forgings, seamless pipe/tube
4This is the maximum design temperature for water service construction. Several ASME Code Cases govern additional usage:
a) Per Section I Code Case 2665, 1300°F (704°C) is the maximum design temperature for molten nitrate salt wetted construction.
b) Per Section I Code Case 2756, autogenous welds can be used in the design range of 1000°F and 1250°F (538-677°C).
c) Weld strength reduction factors are governed by Section I PG-26 and Code Case 2805.
5Section VIII Division 1 Code Case 2671 contains an external pressure chart for 1800°F (982°C).
6For any bolts created from this material, 1650°F is the maximum design temperature. See Section VIII Division 1 Code Case 2775.
7B16 Case 5 allows for higher pressure-temperature ratings for valves made of this material.

Disclaimer

Haynes International makes all reasonable efforts to ensure the accuracy and correctness of the data displayed on this site but makes no representations or warranties as to the data’s accuracy, correctness or reliability. All data are for general information only and not for providing design advice. Alloy properties disclosed here are based on work conducted principally by Haynes International, Inc. and occasionally supplemented by information from the open literature and, as such, are indicative only of the results of such tests and should not be considered guaranteed maximums or minimums.  It is the responsibility of the user to test specific alloys under actual service conditions to determine their suitability for a particular purpose.

For specific concentrations of elements present in a particular product and a discussion of the potential health affects thereof, refer to the Safety Data Sheets supplied by Haynes International, Inc.  All trademarks are owned by Haynes International, Inc., unless otherwise indicated.

Alloy Brochure

Footer