HAYNES® 556®

Principal Features

HAYNES® 556® alloy (UNS R30556) is an iron-nickel-chromium-cobalt alloy that combines effective resistance to sulfidizing, carburizing and chlorine-bearing environments at high temperatures with good oxidation resistance, fabricability, and excellent high-temperature strength. It has also been found to resist corrosion by molten chloride salts and other salts, and is resistant to corrosion from molten zinc.

Ease of Fabrication

HAYNES® 556® alloy has excellent forming and welding characteristics. It may be forged or otherwise hot-worked, providing that it is held at 2150°F (1175°C) for a time sufficient to bring the entire piece to temperature. As a consequence of its good ductility, 556® alloy is also readily formed by cold working. All hot- or cold-worked parts should be annealed and rapidly cooled in order to restore the best balance of properties.

The alloy can be welded by a variety of techniques, including gas tungsten arc (GTAW), gas metal arc (GMAW), shielded metal arc (coated electrode), and resistance welding.

Heat Treatment

HAYNES® 556® alloy is furnished in the solution heat treated condition, unless otherwise specified. The alloy is normally solution heat treated at 2150°F (1175°C) and rapidly cooled or water-quenched for optimum properties. Heat treatments at temperatures lower than the solution heat-treating temperature may cause precipitation of secondary phases.

Applications

HAYNES® 556® alloy combines properties which make it highly useful for service at elevated-temperature in moderately to severely corrosive environments. Applications can include tubing and structural members in municipal and industrial waste incinerators, rotary calciners and kilns for minerals processing, and non-rotating components in industrial gas turbines burning low-grade fuels.

In the chemical process industry, 556® alloy is used for applications in rotary calciners, carbon regenerators, and in processes involving high-sulfur petroleum feedstocks.

In the metallurgical process industry, 556® alloy is widely used for hot-dip galvanizing fixtures, spinners and baskets, and for high speed furnace fans. 556® alloy is also employed in air preheaters of diesel engines, the inner covers of coil annealing furnaces, and in various high-temperature applications in the aerospace industry.

*Please contact our technical support team if you have technical questions about this alloy.

Nominal Composition

Weight %
Iron 31 Balance
Nickel 20
Cobalt 18
Chromium 22
Molybdenum 3
Tungsten 2.5
Tantalum 0.6
Nitrogen 0.2
Silicon 0.4
Niobium 0.3 max.
Manganese 1
Aluminum 0.2
Carbon 0.1
Boron 0.02 max.
Lanthanum 0.02
Zirconium 0.02

Sulfidation Resistance

HAYNES® 556® alloy is second in resistance only to HAYNES® HR-160® alloy to the types of sulfur-bearing environments that are present in many high-temperature industrial processes. This is due partly to its comparatively low nickel content coupled with the important addition of cobalt, the high chromium level, and the carefully balanced minor elements. For comparison, data illustrating the relative sulfidation resistance of INCONEL® alloy 601, HASTELLOY® X alloy, alloys 600 and 800H, and Type 310 stainless steel are shown in the accompanying photomicrographs. 556® alloy had little sulfide penetration or wastage after 215 hours of exposure in an Ar+5%H2+5%CO+1%CO2+ 0.15%H2S+0.1%H2O test gas at 1800°F (980°C). By contrast, alloys such as INCONEL® alloy 601 were completely destroyed, while other materials suffered severe wastage and sulfide penetration or pitting.

Comparative Sulfidation Resistance at 1800°F (980°C) for 215 Hours

HAYNES® 556® alloy

Average Metal Affected = 2.0 Mils (50 μm)/Side

Type 310 Stainless Steel

Average Metal Affected = 7.4 Mils (190μm)/Side

Alloy 800H

Average Metal Affected = 23.2 Mils (590μm)/Side

HASTELLOY® X alloy

Average Metal Affected = > 22 Mils (560 μm)/Side

INCONEL alloy 601

Average Metal Affected = > 22 Mils (560 μm)/Side

alloy 600

Average Metal Affected = > 22 Mils (560 μm)/Side

Sulfidation Resistance at Other Temperatures

Alloy 1400°F (760°C) 1600°F (871°C)
Metal Loss Average Metal Affected** Metal Loss Average Metal Affected**
– mils µm mils µm mils µm mils µm
HR-160® 0.2 5 1.1 30 0.1 3 3.8 95
556® 2.5 65 3.8 95 5.2 130 11.7 295
Type 310 6.2 155 9.2 230 9.5 240 13.5 345
800H 7.1 180 11.2 285 11.7 295 19.2 490
X >29.5 >750 Perforated >21.7 >550 Consumed
600 >21.7 >560 Perforated >21.7 >550 Consumed
601 >29.5 >750 Perforated >21.7 >550 Perforated

*215 Hour Exposure in Ar+5% H2 +5%CO+1% CO2 +0.15%H2 S+0.10%H2O **Metal Loss + Average Internal Penetration.

Field Experience – Municipal Waste Incinerator

Samples were exposed for 950 hours in the superheater section of a municipal waste incinerator. Combustion gas temperatures were about 1475°F (800°C) with excursions to 1740°F (950°C). The mode of corrosion observed was oxidation/sulfidation, although alkali chloride compounds were known to be present. HAYNES® 556® alloy was found to be one of the best alloys for resisting this highly corrosive environment.

Field Experience – Aluminum Remelting Furnace

Samples of tubing were exposed for 1150 hours in the recuperator of an aluminum remelting furnace producing 1250°F (675°C) flue gases. The tube samples were internally cooled by combustion preheat air the same as the operating recuperator tubes. The mode of corrosion observed was combined attack by alkali sulfates and chlorides together with oxidation. HAYNES® 556® alloy exhibited outstanding resistance to corrosion in this environment.

Carburization Resistance

HAYNES® 556® alloy has excellent resistance to carburization, as measured in both mixed gas exposure tests and packed graphite exposure tests. Results for these tests are presented in the following pages.

All results are presented in terms of the mass of carbon absorption per unit area, which was obtained from the equation M = C(W/A) where M = the mass of carbon absorption per unit area (mg/cm2). C = difference in carbon (weightfraction) before and after exposure, W = weight of the unexposed specimen (mg) and A = surface area of the specimen exposed to the test environment (cm2).

Packed Carburization Resistance

Carbon absorption observed for 556® alloy following 500 hour exposure in packed graphite at 1800°F (980°C) was negligible, as shown below. Similar resistance was exhibited by HAYNES® HR-120® alloy. This is in contrast to other alloys tested, all of which exhibited measurable carbon absorption. In particular, the resistance to carburization of 556® alloy was significantly better than that for the stainless steel type materials.

Mix Gas Carburization Tests

Carbon absorption observed for 556® alloy following exposure at both 1700°F (925°C) and 1800°F (980°C) to a carburizing gas mixture was significantly lower than that for most other materials tested. This is shown in the graphs on the following pages. For these tests, the exposure was performed in a gas environment consisting of (by volume %) 5.0% H2, 5.0% CO, 5.0% CH4 and the balance argon. The calculated equilibrium composition (volume %) at 1800°F (980°C) and one atm was 14.2% H2, 4.8% CO, 0.003% CO2, 0.026% CH4, 0.011% H2O and the balance argon. The activity of carbon was 1.0 and the partial pressure of oxygen was 9 x 10-22 atm at 1800°F (980°C).

Comparative 1700°F (925°C) Mix Gas Carburization Tests

Typical Carburized Microstructures (Unetched) After Exposure
For 215 Hours at 1700°F (925°C)

HAYNES® 556® alloy

Type 310 Stainless Steel

Comparative 1800°F (980°C) Mix Gas Carburization Tests

Typical Carburized Microstructures (Unetched) After Exposure
For 55 Hours at 1800°F (980°C)

HAYNES® 556® alloy

INCONEL alloy 617
Note: Alloy 617 is carburized to the center of the sample.

Oxidation Resistance

HAYNES® 556® alloy exhibits good resistance to both air and combustion gas oxidizing environments, and can be used for long-term exposure at temperatures up to 2000°F (1095°C). For exposures of short duration, 556® alloy can be used at higher temperatures.

Comparative Oxidation Resistance in Flowing Air*

Comparative Oxidation Resistance in Flowing Air*, 1008 Hours
Alloy 1800°F (980°C) 2000°F (1095°C)
Average Metal Affected** Metal Loss Average Metal Affected** Metal Loss
- mils µm mils µm mils µm mils µm
X 1.5 38 0.2 5 4.4 112 1.3 33
601 1.7 43 0.4 10 3.8 97 1.3 33
556® 2.3 58 0.4 10 6.9 175 1.5 38
446 SS 2.3 60 1.3 35 14.4 366 13.0 330
RA330 3.0 76 0.3 8 6.7 170 0.8 20
800HT 4.1 104 0.5 13 11.6 295 7.6 193
304 SS 8.1 206 5.5 140 > 19.6 > 498 N/A N/A
316 SS 14.2 361 12.3 312 > 17.5 > 445 N/A N/A

*Flowing air at a velocity of 7.0 ft/min (213.4 cm/min) past the samples.
Samples cycled to room temperature once per week.
**Average Metal Affected = Metal Loss + Average Internal Penetration

Metallographic Technique used for Evaluating Environmental Tests

Comparative Oxidation in Flowing Air 1800°F (980°C) for 1008 Hours

Microstructures shown are for coupons exposed for 1008 hours at 1800°F (980°C) in air flowing 7.0 feet/minute (212.0 cm/minute) past the samples. Samples were descaled by cathodically charging the coupons while they were immersed in a molten salt solution. The black area shown at the top of each picture represents actual metal loss due to oxidation. The data clearly show HAYNES® 556® alloy to be superior to both RA330® alloy and Type 304 stainless steel as well as the other iron-base alloys shown in the table on the previous page.

HAYNES® 556® alloy
Average Metal Affected
= 2.3 mils (58 µm)

RA330 alloy
Average Metal Affected
= 3.0 mils (76 µm)

Type 304 Stainless Steel
Average Metal Affected
= 8.1 mils (206 µm)

Oxidation Test Parameters

Burner rig oxidation tests were conducted by exposing, in a rotating holder, samples 0.375 inch x 2.5 inches x thickness (9.5mm x 64mm x thickness) to the products of combustion of fuel oil (2 parts No. 1 and 1 part No. 2) burned at a ratio of air to fuel of about 50:1. (Gas velocity was about 0.3 mach). Samples were automatically removed from the gas stream every 30 minutes and fan cooled to less than 500°F (260°C) and then reinserted into the flame tunnel.

Comparative Dynamic Oxidation

Alloy 1600°F (870°C), 2000 h, 30-min cycles 1800°F (980°C), 1000 h, 30-min cycles 2000°F (1090°C), 500 h, 30-min cycles 2100°F (1150°C), 200 h, 30-min cycles
Metal Loss Average Metal Affected Metal Loss Average Metal Affected Metal Loss Average Metal Affected Metal Loss Average Metal Affected
- mils µm mils µm mils µm mils µm mils µm mils µm mils µm mils µm
188 1.1 28 2.9 74 1.1 28 3.2 81 10.9 277 13.1 333 8 203 9.7 246
230 0.9 23 3.9 99 2.8 71 5.6 142 7.1 180 9.9 251 6.4 163 13.1 333
617 2 51 7.8 198 2.4 61 5.7 145 13.3 338 20.9 531 13.8 351 15.3 389
625 1.2 30 2.2 56 3.7 94 6 152 – – Consumed – – – –
556® 1.5 38 3.9 99 4.1 104 6.7 170 9.9 251 12.1 307 11.5 292 14 356
X 1.7 43 5.3 135 4.3 109 7.3 185 11.6 295 14 356 13.9 353 15.9 404
HR-120® – – – – 6.3 160 8.3 211 – – – – – – – –
RA330 2.5 64 5 127 8.7 221 10.5 267 15.4 391 17.9 455 11.5 292 13 330
HR-160® – – – – 5.4 137 11.9 302 12.5 18.1 460 8.7 221 15.5 394
310SS 6 152 7.9 201 16 406 18.3 465 – – – – – – Consumed
800H 3.9 99 9.4 239 22.9 582 Through Thickness – – Consumed after 300 h – – Consumed

Amount of metal affected for high‐temperature sheet (0.060 ‐0.125”) alloys exposed for 360 days (8,640‐h) in flowing air.*

Alloy 1600°F (870°C) 1800°F (980°C) 2000°F (1090°C)
Metal Loss** Average Metal Affected*** Metal Loss** Average Metal Affected*** Metal Loss** Average Metal Affected***
- mils µm mils µm mils µm mils µm mils µm mils µm
230® 0.2 5 1.4 36 0.1 3 2.5 64 3.4 86 11 279
HR-120® 0.3 8 1.6 41 0.5 13 3.3 84 18.1 460 23.2 589
188 0.2 5 1.8 46 – – – – – – – –
556® 0.3 8 1.9 48 0.5 13 6.2 157 15 381 24.1 612
X 0.3 8 2.2 56 0.2 5 2.8 71 17.1 434 26.2 665
800HT 0.4 10 2.9 74 – – – – – – – –

*Flowing air at a velocity of 7.0 ft/min (213.4 cm/min) past the samples.  Samples cycled to room temperature once per month.
** Metal loss was calculated from final and initial metal thicknesses; i.e. ML = (OMT – FMT) /2
***Average Metal Affected is sum of Metal Loss and Average Internal Penetration

Resistance to Chlorine-Bearing Environments

HAYNES® 556® alloy can be considered resistant to high-temperature oxidizing environments containing chlorine. Although not as resistant as HAYNES® 214® alloy at temperatures above 1650°F (900°C), 556 alloy has resistance comparable to that of 214® alloy at temperatures at or below 1650°F (900°C). This is shown by the test results given for 400 hour exposures at 1650°F (900°C) in a flowing gas mixture of Ar+20%O2+0.25% Cl2. Note that 556® alloy shows very low metal loss compared to most of the alloys tested, which included alloys 600, 625, INCONEL alloy 601 and HASTELLOY® C-276 alloy.

Other Environments

HAYNES® 556® alloy exhibits reasonable resistance to neutral NaCl-KCl-BaCl2 type heat-treating salts at temperatures up to 1550°F (845°C) based upon actual field tests in a molten salt pot heat treating facility. Coupons were exposed for 30 days.

Alloy Average Metal Affected
– mils mm
188 28 0.7
X 38 1.0
556® 42 1.1
304 SS 74 1.9
310 SS 79 2.0
600 94 2.4
INCONEL® 601 115 2.9

Phosphorus-Bearing Combustion Environment

Based upon field tests performed in the combustion chamber of a fluid bed dryer used to dry sodium tripolyphosphate compounds, HAYNES® 556® alloy exhibits very good resistance to corrosion caused by formation of low-melting point eutectics involving phosphorus. Samples were exposed 30 days at a temperature of about 1475°F (800°C).

Alloy Average Metal Affected
– mils mm
X 3.0 75
556® 6.0 150
214® 8.0 205
S 9.0 230
188 9.0 230
800H 11.0 280
304 SS 15.0 380

Molten Zinc

Resistance to molten zinc is an important consideration for structural components in galvanizing operations. Laboratory tests were performed at 850°F (455°C) for 50 hours in molten zinc to determine suitability for such operations. Results are given below:

Alloy Average Metal Affected
– mils mm
556® 1.6 41
25 2.3 58
188 64 2.5
1010 Carbon Steel 234 9.2
446 SS 236 9.3
Alloy Average Metal Affected
– mils mm
800H 11.0 280
304 SS 14.1 358
625 >24.0** >610**
X >24.0** >610**

*No internal attack noted for any of the alloys tested

Physical Properties

Physical Property Customary Units Metric Units
Density RT
0.297 lb/in3
RT
8.23 g/cm3
Melting Temperature 2425-2580°F - 1330-1415°C -
Electrical Resistivity RT 35.7 µohm-in RT 95.2 µohm-cm
200°F 38.7 µohm-in 100°C 98.6 µohm-cm
400°F 40.5 µohm-in 200°C 102.6 µohm-cm
600°F 42.1 µohm-in 300°C 106.5 µohm-cm
800°F 43.5 µohm-in 400°C 109.5 µohm-cm
1000°F 44.7 µohm-in 500°C 112.5 µohm-cm
1200°F 45.7 µohm-in 600°C 115.1 µohm-cm
1400°F 46.6 µohm-in 700°C 117.2 µohm-cm
1600°F 47.3 µohm-in 800°C 119.0 µohm-cm
1800°F 48.0 µohm-in 900°C 120.7 µohm-cm
2000°F 48.6 µohm-in 1000°C 122.3 µohm-cm
– – 1100°C 123.7 µohm-cm
Thermal Diffusivity RT
4.5 x 10-3 in2/s
RT
28.7 x 10-3cm2/s
200°F
4.8 x 10-3 in2/s
100°C
31.2 x 10-3cm2/s
400°F
5.3 x 10-3 in2/s
200°C
34.2 x 10-3cm2/s
600°F
5.8 x 10-3 in2/s
300°C
37.0 x 10-3cm2/s
800°F
6.3 x 10-3 in2/s
400°C
39.7 x 10-3cm2/s
1000°F
6.7 x 10-3 in2/s
500°C
42.3 x 10-3cm2/s
1200°F
7.1 x 10-3 in2/s
600°C
44.8 x 10-3cm2/s
1400°F
7.5 x 10-3 in2/s
700°C
47.0 x 10-3cm2/s
1600°F
7.7 x 10-3 in2/s
800°C
48.8 x 10-3cm2/s
1800°F
8.0 x 10-3 in2/s
900°C
50.3 x 10-3cm2/s
2000°F
8.2 x 10-3 in2/s
1000°C
51.6 x 10-3cm2/s
- - 1100°C
52.8 x 10-3cm2/s
Thermal Conductivity RT
77 Btu-in/ft2-hr-°F
RT 11.1 W/m-°C
200°F
90 Btu-in/ft2-hr-°F
100°C 13.1 W/m-°C
400°F
107 Btu-in/ft2-hr-°F
200°C 15.4 W/m-°C
600°F
122 Btu-in/ft2-hr-°F
300°C 17.3 W/m-°C
800°F
135 Btu-in/ft2-hr-°F
400°C 19.0 W/m-°C
1000°F
148 Btu-in/ft2-hr-°F
500°C 20.8 W/m-°C
1200°F
160 Btu-in/ft2-hr-°F
600°C 22.4 W/m-°C
1400°F
173 Btu-in/ft2-hr-°F
700°C 24.0 W/m-°C
1600°F
185 Btu-in/ft2-hr-°F
800°C 25.5 W/m-°C
1800°F
197 Btu-in/ft2-hr-°F
900°C 27.2 W/m-°C
2000°F
210 Btu-in/ft2-hr-°F
1000°C 28.9 W/m-°C
- - 1100°C 30.4 W/m-°C
Specific Heat RT 0.111 Btu/lb-°F RT 464 J/kg·°C
200°F 0.113 Btu/lb-°F 100°C 475 J/kg·°C
400°F 0.118 Btu/lb-°F 200°C 493 J/kg·°C
600°F 0.122 Btu/lb-°F 300°C 508 J/kg·°C
800°F 0.126 Btu/lb-°F 400°C 523 J/kg·°C
1000°F 0.130 Btu/lb-°F 500°C 538 J/kg·°C
1200°F 0.133 Btu/lb-°F 600°C 552 J/kg·°C
1400°F 0.135 Btu/lb-°F 700°C 561 J/kg·°C
1600°F 0.140 Btu/lb-°F 800°C 570 J/kg·°C
1800°F 0.147 Btu/lb-°F 900°C 595 J/kg·°C
2000°F 0.152 Btu/lb-°F 1000°C 618 J/kg·°C
- - 1100°C 638 J/kg·°C
Mean Coefficient of Thermal Expansion 70-200°F 8.1 µin/in -°F 25-100°C
14.7 x 10-6m/m·°C
70-400°F 8.2 µin/in -°F 25-200°C
14.9 x 10-6m/m·°C
70-600°F 8.4 µin/in -°F 25-300°C
15.1 x 10-6m/m·°C
70-800°F 8.6 µin/in -°F 25-400°C
15.4 x 10-6m/m·°C
70-1000°F 8.8 µin/in -°F 25-500°C
15.7 x 10-6m/m·°C
70-1200°F 9.0 µin/in -°F 25-600°C
16.1 x 10-6m/m·°C
70-1400°F 9.2 µin/in -°F 25-700°C
16.4 x 10-6m/m·°C
70-1600°F 9.4 µin/in -°F 25-800°C
16.7 x 10-6m/m·°C
70-1800°F 9.5 µin/in -°F 25-900°C
17.0 x 10-6m/m·°C
70-2000°F 9.6 µin/in -°F 25-1000°C
17.1 x 10-6m/m·°C
- - 25-1100°C
17.1 x 10-6m/m·°C
Dynamic Modulus of Elasticity RT
29.7 x 106 psi
RT 205 GPa
200°F
29.1 x 106 psi
100°C 200 GPa
400°F
28.2 x 106 psi
200°C 195 GPa
600°F
26.9 x 106 psi
300°C 187 GPa
800°F
25.6 x 106 psi
400°C 179 GPa
1000°F
24.4 x 106 psi
500°C 172 GPa
1200°F
23.1 x 106 psi
600°C 164 GPa
1400°F
21.8 x 106 psi
700°C 155 GPa
1600°F
20.9 x 106 psi
800°C 148 Gpa
1800°F
20.1 x 106 psi
900°C 143 Gpa
- - 1000°C 138 Gpa

RT= Room Temperature

Applications

Tensile Properties

Cold-Rolled and Solution-annealed Sheet, 0.033 to 0.109 in. (0.8 to 2.8 mm) Thick*

Test Temperature 0.2% Yield Strength Ultimate Tensile Strength Elongation
°F °C ksi MPa ksi MPa %
RT RT 59.5 410 118.1 815 47.7
1000 538 34.9 240 93.4 645 54.4
1200 649 32.8 225 85.4 590 52.4
1400 760 32.0 220 68.5 470 49.1
1600 871 28.6 195 47.6 330 52.6
1800 982 15.5 105 28.0 195 63.3
2000 1093 8.0 55 14.8 100 55.4

*Based upon 10 or more Tests per condition
RT= Room Temperature

Elevated temperature tensile tests for sheet were performed with a strain rate that is no longer standard.  These results were from tests with a strain rate of 0.005 in./in./minute through yield and a crosshead speed of 0.5 in./minute for every inch of reduced test section from yield through failure. The current standard is to use a strain rate of 0.005 in./in./minute though yield and a crosshead speed of 0.05 in./minute for every inch of reduced test section from yield through failure.

Comparative Yield Strengths (Sheet)

Holt-Rolled and Solution-annealed Plate

Test Temperature 0.2% Yield Strength Ultimate Tensile Strength Elongation
°F °C ksi MPa ksi MPa %
RT RT 54.1 373 114.6 790 51.3
1000 538 33.7 232 95.6 659 58.2
1200 649 33.2 229 87.2 601 55.1
1400 760 34.0 234 63.1 435 57.4
1600 871 26.9 185 37.4 258 87.9
1800 982 13.2 91 20.3 140 96.2
2000 1093 6.7 46 11.2 77 90.3

RT= Room Temperature

Creep and Rupture Properties

Solution Annealed Sheet, Plate and Bar

Test Temperature Creep Approximate Initial Stress to Produce Specified Creep in:
10 h 100 h 1000 h 10,000 h*
°F °C % ksi MPa ksi MPa ksi MPa ksi MPa
1200 650 0.5 44.0 305 32.0 220 24.0 165 – –
1.0 49.0 340 35.0 240 25.5 175 18.5 130
Rupture – – 53.0 365 38.0 260 27.5 190
1300 705 0.5 29.0 200 21.0 145 15.0 105 – –
1.0 33.0 230 24.0 165 17.5 120 12.5 86
Rupture 52.0 360 37.0 255 26.0 180 17.0 115
1400 760 0.5 19.0 130 13.5 93 9.4 65 – –
1.0 22.0 150 16.0 110 11.5 79 8.5 59
Rupture 35.0 240 25.0 170 17.5 120 11.9 82
1500 815 0.5 13.0 90 9.0 62 6.5 45 – –
1.0 15.0 105 11.0 76 8.2 57 6.0 41
Rupture 25.0 170 17.0 115 11.8 81 7.6 52
1600 870 0.5 8.9 61 6.4 44 4.6 32 – –
1.0 10.0 69 7.5 52 5.5 38 4.1 28
Rupture 17.0 115 11.5 79 7.5 52 4.9 34<
1700 925 0.5 6.2 43 4.5 31 3.2 22 – –
1.0 7.2 50 5.0 34 3.5 24 2.5 17
Rupture 12.0 83 7.6 52 4.8 33 3.0 21
1800 980 0.5 4.4 30 3.0 21 2.0 14 – –
1.0 5.0 34 3.4 23 2.3 16 1.6 11
Rupture 7.5 52 4.8 33 3.0 21 1.9 13

Impact Properties

Alloy V-Notch Impact Strength1 Room Temperature
– ft.-lb. J
800H 2392 3242
600 180 244
556® 1772 2402
188 143 194
S 140 190
625 81 110
X 54 73

1 Average of 4 or more tests
2 Samples did not break

Thermal Stability

HAYNES® 556® exhibits reasonable retained ductility after long term thermal exposure at intermediate temperatures. It does not exhibit significant sigma phase formation even after 16,000 hours exposure at 1000 to 1600°F(540 to 870°C). Principal phases precipitated from solid solution are carbides and carbonitrides.

Room-Temperature Tensile Properties of Bar Following Thermal Exposure*

Test Temperature – 0.2% Yield Strength Ultimate Tensile Strength Elongation
°F °C h ksi MPa ksi MPa %
1200 650 0 62.5 430 113.4 780 46.5
1000 59.7 410 120.5 830 36.0
4000 57.4 395 121.2 835 33.0
8000 59.8 410 127.3 880 29.4
1400 760 0 62.5 430 113.4 780 46.5
1000 60.8 420 128.7 885 24.8
4000 57.4 395 127.1 875 25.8
8000 54.6 375 125.1 865 24.7
1600 870 0 62.5 430 113.4 780 46.5
1000 52.3 360 112.9 780 32.8
4000 42.8 295 111.5 770 29.0
8000 43.9 305 108.1 745 29.5

*Average of three tests for each condition

Elevated-Temperature Tensile Properties of
Bar Following 16,000-Hour Thermal Exposures*

Test Temperature 0.2% Yield Strength Ultimate Tensile Strength Elongation
°F °C ksi MPa ksi MPa %
1000 537 37.4 260 95.7 660 48.0
1200 648 37.8 260 88.8 610 23.4
1400 760 35.1 240 72.3 500 25.3
1600 871 21.9 150 42.1 290 29.5

Room-Temperature Tensile Properties of
Sheet Following 1000-Hour Thermal Exposures*

Exposure Temperature 0.2% Yield Strength Ultimate Tensile Strength Elongation
°F °C ksi MPa ksi MPa %
None None 59.5 410 118.1 815 47.7
1200 648 53.4 370 118.4 815 37.9
1400 760 53.8 370 118.8 820 17.0
1600 871 46.6 320 111 765 20.4

Fabrication Characteristics

HAYNES® 556® alloy is normally final solution heat-treated at 2150°F (1175°C) for a time commensurate with section thickness. Solution heat-treating can be performed at temperatures as low as about 2125°F (1165°C), but resulting material properties will be altered accordingly. Annealing during fabrication can be performed at even lower temperatures, but a final, subsequent solution heat treatment is needed to produce optimum properties and structure. Please click here or see the Haynes Welding SmartGuide for more information.

Typical Hardness Properties

Form Hardness, HRBW Typical ASTM Grain Size
Sheet 91 4 – 6.5
Plate 92 3.5 – 6.5
Bar 89 3 – 5.5

All samples tested in solution-annealed condition.
HRBW = Rockwell Hardness «B», Tungsten Indentor.

Effect of Cold Reduction upon Room Temperature Tensile Properties*

Cold Reduction Subsequent Anneal Temperature 0.2% Yield Strength Ultimate Tensile Strength Elongation
% - ksi MPa ksi MPa %
0 None 52.9 365 115.0 795 50.7
10 93.3 645 127.8 880 34.8
20 113.3 780 142.1 980 23.5
30 144.1 995 172.6 1190 12.0
40 155.8 1075 189.3 1305 10.1
50 169.7 1170 204.2 1410 8.0
0 1850°F (1010°C) 52.6 365 114.7 790 44.8
10 76.9 530 121.6 840 34.3
20 88.8 610 127.0 875 30.3
30 92.7 340 135.2 930 26.6
40 80.0 550 133.3 920 30.6
50 83.0 570 135.0 930 31.7
0 1950°F (1065°C) 52.9 365 115.8 800 45.2
10 76.8 530 122.2 845 36.9
20 76.8 530 124.7 860 34.8
30 66.0 455 125.1 865 38.3
40 71.4 490 128.1 885 36.7
50 77.9 535 131.0 905 33.4
0 2050°F (1121°C) 54.3 375 117.0 805 47.0
10 55.3 380 117.4 810 48.0
20 58.4 405 120.1 830 45.4
30 63.5 440 123.6 850 43.0
40 66.9 460 124.7 860 42.4
50 70.8 485 126.6 875 35.0

* Based upon rolling reductions taken upon 0.120-inch (3.0mm) thick sheet. Duplicate tests.

Typical Microstructure
(ASTM 5 grain size) Annealed at 2150°F (1175°C)

Etchant:95ml
HCL plus 5gm oxalic acid, 4 volts

Welding

HAYNES® 556® alloy is readily welded by Gas Tungsten Arc (GTAW), Gas Metal Arc (GMAW), Shielded Metal Arc (SMAW), and resistance welding techniques.  Submerged Arc welding is not recommended, as this process is characterized by high heat input to the base metal and slow cooling of the weld.  These factors can increase weld restraint and promote cracking.

Base Metal Preparation

The joint surface and adjacent area should be thoroughly cleaned before welding.  All grease, oil, crayon marks, sulfur compounds, and other foreign matter should be removed.  Contact with copper or copper-bearing materials in the joint area should be avoided.  It is preferable, but not necessary, that the alloy be in the solution-annealed condition when welded.

Filler Metal Selection

Matching composition filler metal is recommended for joining 556® alloy. For shielded metal-arc welding, MULTIMET® electrodes (AMS 5795) are suggested. For dissimilar metal joining of 556® alloy to nickel- or cobalt-base materials, 556® filler metal will generally be a good selection, but HASTELLOY® S alloy (AMS 5838) or HASTELLOY® W alloy (AMS 5786, 5787) welding products may be used. For dissimilar welding to iron-base materials, 556® filler metal is recommended. Please click here or the Haynes Welding SmartGuide for more information.

Preheating, Interpass Temperatures, and Postweld Heat Treatment

Preheat is not required. Preheat is generally specified as room temperature (typical shop conditions).   Interpass temperature should be maintained below 200°F (93°C). Auxiliary cooling methods may be used between weld passes, as needed, providing that such methods do not introduce contaminants.  Postweld heat treatment is not generally required for 188 alloy.  For further information, please click here.

Typical Tensile Properties

Condition Test Temperature 0.2% Yield Strength Ultimate Tensile Strength Elongation
- °F °C ksi MPa ksi MPa %
Transverse Tensile RT RT 63.6 439 120.6 832 42.8
1000 540 41.1 283 95.6 659 50.3
1200 650 38.3 264 84.8 585 47.6
1400 760 34.1 235 63.1 435 44.8
All Weld Metal RT RT 67.3 464 107.3 739 43.1
1200 650 44.6 308 71.4 492 39.4
1400 760 42.4 292 55.2 381 55.2

Typical crack-free face and root bends for welded HAYNES® 556® alloy
0.5 inch (13 mm) plate and matching filler metal.
Bend radius was 0.75 inch (19 mm).

Specifications and Codes

Specifications

HAYNES® 556® alloy (R30556)
Sheet, Plate & Strip AMS 5874 SB 435/B 435 P= 45
Billet, Rod & Bar AMS 5877 SB 572/B 572 B 472 P= 45
Coated Electrodes –
Bare Welding Rods & Wire SFA 5.9/ A 5.9 (ER3556) AMS 5831 F= 6
Seamless Pipe & Tube SB 622/B 622 P= 45
Welded Pipe & Tube SB 619/B 619SB 626/B 626 P= 45
Fittings SB 366/B 366 P= 45
Forgings AMS 5877
DIN No. 1.4883X10 CrNiCoMoN22 20 18
Others –

Codes

HAYNES® 556® alloy (R30556)
ASME Section l –
Section lll Class 1 –
Class 2 –
Class 3 –
Section lV HF-300.2
Section Vlll Div. 1
1650°F (899°C)14
Div. 2
800°F (427°C)19
Section Xll
650°F (343°C)5
B16.5
1500°F (816°C)20
B16.34
1500°F (816°C)20
B31.1
1200°F (649°C)2
B31.3 –

1Plate, Sheet, Bar, welded pipe/tube, seamless pipe/tube
2Bolting
3Plate, Sheet, Bar, welded pipe/tube, seamless pipe/tube
4Plate, Bar
5Plate, Sheet, Bar, fittings, welded pipe/tube, seamless pipe/tube

Disclaimer

Haynes International makes all reasonable efforts to ensure the accuracy and correctness of the data displayed on this site but makes no representations or warranties as to the data’s accuracy, correctness or reliability. All data are for general information only and not for providing design advice. Alloy properties disclosed here are based on work conducted principally by Haynes International, Inc. and occasionally supplemented by information from the open literature and, as such, are indicative only of the results of such tests and should not be considered guaranteed maximums or minimums.  It is the responsibility of the user to test specific alloys under actual service conditions to determine their suitability for a particular purpose.

For specific concentrations of elements present in a particular product and a discussion of the potential health affects thereof, refer to the Safety Data Sheets supplied by Haynes International, Inc.  All trademarks are owned by Haynes International, Inc., unless otherwise indicated.