Principal Features
STELLITE® alloy-like wear resistance and HASTELLOY® alloy-like corrosion resistance in a single, highly weldable material
ULTIMET® alloy (UNS R31233) provides a unique blend of properties. From a wear standpoint, it behaves like the STELLITE® alloys with lower carbon contents. From a corrosion standpoint, it possesses many of the attributes of the C-type and G-type HASTELLOY® materials, in particular outstanding resistance to chloride-induced pitting and crevice corrosion. Its mechanical and welding characteristics are much closer to those of the HASTELLOY® alloys than those of the STELLITE® alloys, whose low ductilities can be problematic.
While ULTIMET® alloy has been used successfully in the form of wrought products, its largest applications have involved weld overlays, made with solid wire consumables and arc-welding processes such as GMAW (MIG) and GTAW (TIG).
*Please contact our technical support team if you have technical questions about this alloy.
Nominal Composition
| Weight % | |
| Cobalt | Balance |
| Chromium | 26 |
| Nickel | 9 |
| Molybdenum | 5 |
| Iron | 3 |
| Tungsten | 2 |
| Manganese | 0.8 |
| Silicon | 0.3 |
| Nitrogen | 0.08 |
| Carbon | 0.06 |
Iso-Corrosion Diagrams
Each of these iso-corrosion diagrams was constructed using numerous corrosion rate values, generated at different acid concentrations and temperatures. The blue line represents those combinations of acid concentration and temperature at which a corrosion rate of 0.1 mm/y (4 mils per year) is expected, based on laboratory tests in reagent grade acids. Below the line, rates under 0.1 mm/y are expected. Similarly, the red line indicates the combinations of acid concentration and temperature at which a corrosion rate of 0.5 mm/y (20 mils per year) is expected. Above the line, rates over 0.5 mm/y are expected. Between the blue and red lines, corrosion rates are expected to fall between 0.1 and 0.5 mm/y.

Comparative 0.1 mm/y Line Plots
To compare the performance of ULTIMET® alloy with that of other materials, it is useful to plot the 0.1 mm/y lines. In the following graphs, the lines for ULTIMET® alloy are compared with those of two popular, austenitic stainless steels (316L and 254SMO), and two nickel alloys (625 and C-22®), in hydrochloric and sulfuric acids. The tests in hydrochloric acid were limited to a concentration of 20% (the azeotrope). At hydrochloric acid concentrations up to 15%, the performance of ULTIMET® alloy exceeds that of alloy 625, and in sulfuric acid, the performance of ULTIMET® alloy matches that of alloy 625 at many concentrations.

Selected Corrosion Data
Hydrochloric Acid
| Conc. Wt.% | 50°F | 75°F | 100°F | 125°F | 150°F | 175°F | 200°F | 225°F | Boiling |
| 10°C | 24°C | 38°C | 52°C | 66°C | 79°C | 93°C | 107°C | ||
| 1 | - | - | - | - | - | - | - | - | <0.05 |
| 1.5 | - | - | - | - | - | - | - | - | - |
| 2 | - | - | - | - | - | - | - | - | - |
| 2.5 | - | - | - | - | <0.01 | <0.01 | <0.01 | - | 43.85 |
| 3 | - | - | - | - | - | - | - | - | - |
| 3.5 | - | - | - | - | - | - | - | - | - |
| 4 | - | - | - | - | - | - | - | - | - |
| 4.5 | - | - | - | - | - | - | - | - | - |
| 5 | - | - | - | - | 0.01 | 5.75 | - | - | - |
| 7.5 | - | - | - | - | - | - | - | - | - |
| 10 | - | <0.01 | 0.16 | 0.80 | 1.74 | - | - | - | - |
| 15 | - | 0.15 | 0.73 | 1.83 | 4.75 | - | - | - | - |
| 20 | - | 0.17 | 0.56 | 1.04 | 2.58 | - | - | - | - |
All corrosion rates are in millimeters per year (mm/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.
Data are from Corrosion Laboratory Job 181-90.
All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.

Nitric Acid
| Conc. Wt.% | 50°F | 75°F | 100°F | 125°F | 150°F | 175°F | 200°F | 225°F | Boiling |
| 10°C | 24°C | 38°C | 52°C | 66°C | 79°C | 93°C | 107°C | ||
| 10 | - | - | - | - | - | - | - | - | <0.01 |
| 20 | - | - | - | - | - | - | - | - | <0.01 |
| 30 | - | - | - | - | - | - | - | - | 0.01 |
| 40 | - | - | - | - | - | - | - | - | 0.03 |
| 50 | - | - | - | - | - | - | - | - | 0.07 |
| 60 | - | - | - | - | - | - | 0.03 | - | 0.12 |
| 65 | - | - | - | - | - | - | 0.04 | - | 0.15 |
| 70 | - | - | - | - | - | - | 0.06 | - | 0.18 |
All corrosion rates are in millimeters per year (mm/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.
Data are from Corrosion Laboratory Job 182-90.
All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.

Phosphoric Acid
| Conc. Wt.% | 125°F | 150°F | 175°F | 200°F | 225°F | 250°F | Boiling |
| 52°C | 66°C | 79°C | 93°C | 107°C | 121°C | ||
| 10 | - | - | - | - | - | <0.01 | |
| 20 | - | - | - | - | - | 0.01 | |
| 30 | - | - | - | - | - | 0.01 | |
| 40 | - | - | - | - | - | 0.03 | |
| 50 | - | - | - | <0.01 | - | - | 0.14 |
| 60 | - | - | - | 0.01 | - | 0.01 | 0.25 |
| 70 | - | - | - | 0.01 | 0.01 | 0.02 | 0.46 |
| 80 | - | - | - | 0.01 | 0.07 | 0.55 | 10.95 |
| 85 | - | - | - | 0.01 | 0.07 | 0.57 | 30.58 |
All corrosion rates are in millimeters per year (mm/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.
Data are from Corrosion Laboratory Job 183-90.
All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.

Sulfuric Acid
| Conc. Wt.% | 75°F | 100°F | 125°F | 150°F | 175°F | 200°F | 225°F | 250°F | 275°F | 300°F | 350°F | Boiling |
| 24°C | 38°C | 52°C | 66°C | 79°C | 93°C | 107°C | 121°C | 135°C | 149°C | 177°C | ||
| 1 | - | - | - | - | - | - | - | - | - | - | - | 0.13 |
| 2 | - | - | - | - | - | <0.01 | - | - | - | - | - | 0.27 |
| 3 | - | - | - | - | - | - | - | - | - | - | - | - |
| 4 | - | - | - | - | - | - | - | - | - | - | - | - |
| 5 | - | - | - | <0.01 | - | 0.01 | - | - | - | - | - | 1.26 |
| 10 | - | - | - | - | - | 0.43 | - | - | - | - | - | 1.92 |
| 20 | - | - | - | <0.01 | 0.01 | 1.83 | - | - | - | - | - | 4.48 |
| 30 | - | - | - | <0.01 | 1.36 | 3.58 | - | - | - | - | - | 10.54 |
| 40 | - | <0.01 | <0.01 | 0.29 | 2.25 | - | - | - | - | - | - | 20.94 |
| 50 | - | <0.01 | - | 0.96 | - | - | - | - | - | - | - | - |
| 60 | - | <0.01 | <0.01 | 1.48 | - | - | - | - | - | - | - | - |
| 65 | - | - | 0.63 | - | - | - | - | - | - | - | - | - |
| 70 | - | <0.01 | 0.55 | - | - | - | - | - | - | - | - | - |
| 80 | - | <0.01 | 1.02 | 1.64 | - | - | - | - | - | - | - | - |
| 85 | - | 0.03 | - | - | - | - | - | - | - | - | - | - |
| 90 | <0.01 | 0.26 | 1.68 | - | - | - | - | - | - | - | - | - |
| 96 | <0.01 | 0.21 | 1.76 | 2.24 | - | - | - | - | - | - | - | - |
All corrosion rates are in millimeters per year (mm/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.
Data are from Corrosion Laboratory Jobs 159-90 and 8-91.
All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.

Reagent Grade Solutions, mm/y
| Chemical | Conc. wt. % | 100°F | 125°F | 150°F | 175°F | 200°F | Boiling |
| 38°C | 52°C | 60°C | 79°C | 93°C | |||
| Acetic Acid | 99 | - | - | - | - | - | <0.01 |
| Hydrochloric Acid | 1 | - | - | - | - | - | 0.05 |
| 2.5 | - | - | <0.01 | <0.01 | <0.01 | 43.85 | |
| 5 | - | - | 0.01 | - | - | - | |
| 10 | 0.16 | 0.80 | 1.74 | - | - | - | |
| 15 | 0.73 | 1.83 | - | - | - | - | |
| 20 | 0.56 | 1.04 | - | - | - | - | |
| Nitric Acid | 10 | - | - | - | - | - | <0.01 |
| 20 | - | - | - | - | - | <0.01 | |
| 30 | - | - | - | - | - | 0.01 | |
| 40 | - | - | - | - | - | 0.03 | |
| 50 | - | - | - | - | - | 0.07 | |
| 60 | - | - | - | - | 0.03 | 0.12 | |
| 65 | - | - | - | - | 0.04 | 0.15 | |
| 70 | - | - | - | - | 0.06 | 0.18 | |
| Phosphoric Acid | 10 | - | - | - | - | - | <0.01 |
| 20 | - | - | - | - | - | 0.01 | |
| 30 | - | - | - | - | - | 0.01 | |
| 40 | - | - | - | - | - | 0.03 | |
| 50 | - | - | - | - | <0.01 | 0.14 | |
| 60 | - | - | - | - | 0.01 | 0.24 | |
| 70 | - | - | - | - | 0.01 | 0.45 | |
| 80 | - | - | - | - | 0.01 | 10.92 | |
| 85 | - | - | - | - | 0.01 | 30.58 | |
| Sulfuric Acid | 1 | - | - | - | - | - | 0.13 |
| 2 | - | - | - | - | <0.01 | 0.27 | |
| 5 | - | - | <0.01 | - | 0.01 | 1.26 | |
| 10 | - | - | - | - | 0.43 | 1.92 | |
| 20 | - | - | <0.01 | 0.01 | 1.83 | - | |
| 30 | - | - | <0.01 | 1.36 | - | - | |
| 40 | <0.01 | <0.01 | 0.29 | 2.25 | - | - | |
| 50 | <0.01 | - | 0.96 | - | - | - | |
| 60 | <0.01 | <0.01 | 1.48 | - | - | - | |
| 70 | <0.01 | 0.55 | - | - | - | - | |
| 80 | <0.01 | 1.02 | - | - | - | - | |
| 90 | 0.26 | 1.68 | - | - | - | - | |
| 96 | 0.21 | 1.76 | - | - | - | - |
Galling Resistance


Erosion Resistance


Abrasion Wear

AWM = All weld metal WO = Weld overlay WRT = Wrought

Resistance to Pitting and Crevice Corrosion
ULTIMET® alloy exhibits very high resistance to chloride-induced pitting and crevice attack, forms of corrosion to which the austenitic stainless steels are particularly prone.
To assess the pitting resistance of ULTIMET® alloy relative to other corrosion-resistant materials, it has been subjected to tests in Green Death (11.5% H2SO4 + 1.2% HCl + 1% FeCl3 + 1% CuCl2). Experiments wereperformed at various temperatures (in increments of 5°C) to determine the lowest temperature at which pitting occurs in a 24 h test period (the so-called Critical Pitting Temperature for Green Death). The results were as follows:
| Alloy | Critical Pitting Temperature | |
| - | °F | °C |
| ULTIMET® | 248 | 120 |
| C-22® | 248 | 120 |
| C-276 | 230 | 110 |
| 625 | 167 | 75 |
| 6B | 113 | 45 |
| 316L | 77 | 25 |
Resistance to Stress Corrosion Cracking
- Wrought ULTIMET alloy has been tested according to NACE TM0177, which defines sulfide stress cracking as a room temperature phenomenon, resulting from hydrogen embrittlement.
- The TM0177 tests involved 5% NaCl + 0.5% glacial acetic acid, saturated with H2S, proof-ring apparatus, and samples coupled to carbon steel and stressed to the point of yield.
- ULTIMET alloy was able to withstand these conditions, both annealed and cold-reduced (15%), indicating good resistance to hydrogen embrittlement.
H2S – Induced Stress Corrosion Cracking
- Cracking at elevated temperatures in environments containing H2S is defined as a form of stress corrosion cracking.
- Wrought ULTIMET alloy has been tested in 20% NaCl + 0.517 MPa (75 psi) H2S + 4.83 MPa (700 psi) CO2, with and without 0.5 g/l sulfur, at 121°C and 177°C; the tests were conducted according to the recommendations of ASTM Standard G 39, the fixtures being made of ULTIMET alloy, to prevent galvanic effects.
- Like other materials, ULTIMET alloy was prone to cracking in the cold-reduced condition, but resistant to H2S-induced stress corrosion cracking in the annealed condition, at these temperatures.
Resistance to Seawater Crevice Corrosion
Seawater is probably the most common aqueous salt solution. Not only is it encountered in marine transportation and offshore oil rigs, but it is also used as a coolant in coastal facilities. Listed are data generated as part of a U.S. Navy study at the LaQue Laboratories in Wrightsville Beach, North Carolina (and published by D.M. Aylor et al, Paper No. 329, CORROSION 99, NACE International, 1999). Crevice tests were performed in both still (quiescent) and flowing seawater, at 29°C, plus or minus 3°C. Two samples (A & B) of each alloy were tested in still water for 180 days, and likewise in flowing water. Each sample contained two possible crevice sites. The results indicate that ULTIMET® alloy is even more resistant to crevice corrosion in seawater than C-276 alloy.
| Alloy | Quiescent | Flowing | ||
| - | No. of Sites Attacked | Maximum Depth of Attack, mm | No. of Sites Attacked | Maximum Depth of Attack, mm |
| 316L | A:2, B:2 | A:1.33, B:2.27 | A:2, B:2 | A:0.48, B:0.15 |
| 254SMO | A:2, B:2 | A:0.76, B:1.73 | A:2, B:2 | A:0.01, B:<0.01 |
| 625 | A:2, B:2 | A:0.18, B:0.04 | A:2, B:2 | A:<0.01, B:<0.01 |
| C-276 | A:1, B:1 | A:0.10, B:0.13 | A:0, B:0 | A:0, B:0 |
| C-22® | A:0, B:0 | A:0, B:0 | A:0, B:0 | A:0, B:0 |
| ULTIMET® | A:0, B:0 | A:0, B:0 | A:0, B:0 | A:0, B:0 |
Corrosion Resistance of Welds
One of the most important product forms of ULTIMET® alloy is welding wire, since many applications involve ULTIMET® weld overlays. These overlays are, of course, subject to dilution from the substrate material, often a steel or stainless steel. To provide some idea of the influence of dilution upon the corrosion resistance of ULTIMET® weld overlays, a study was undertaken whereby pre-diluted consumables were made by the aspiration casting process, and all-weld-metal (AWM) samples made by deposition on chilled copper blocks. Thus, it was possible to conduct regular (rather than one-sided) corrosion tests in acid solutions on homogeneous samples, diluted with specific substrate materials.
| ULTIMET® Alloy | Corrosion Rate, mm/y | ||
| 3% HCl, 66°C (150°F) |
Boiling 65% HNO3 |
Boiling 2% H2SO4 |
|
| Undiluted | 0.68 | 0.15 | 0.41 |
| Diluted with 9.1%/G10400 | 1.80 | 0.30 | 0.69 |
| Diluted with 9.1%/S31603 | 1.42 | 0.25 | 0.58 |
| Diluted with 16.7%/G10400 | 2.13 | 0.30 | 0.84 |
| Diluted with 16.7%/S31603 | 2.08 | 0.23 | 0.48 |
Physical Properties
| Physical Property | Customary Units | Metric Units | ||
| Density | RT |
0.306 lb/in.3 |
RT |
8.47 g/cm.3 |
| Electrical Resistivity | RT | 34.3 µohm.in | RT | 0.87 µohm.m |
| 200°F | 35.2 µohm.in | 100°C | 0.89 µohm.m | |
| 400°F | 36.7 µohm.in | 200°C | 0.93 µohm.m | |
| 600°F | 38.2 µohm.in | 300°C | 0.96 µohm.m | |
| 800°F | 39.6 µohm.in | 400°C | 1.00 µohm.m | |
| 1000°F | 40.9 µohm.in | 500°C | 1.03 µohm.m | |
| - | - | 600°C | 1.05 µohm.m | |
| Thermal Conductivity | RT |
87 Btu.in/h.ft2.°F |
RT | 12.3 W/m.°C |
| 200°F |
95 Btu.in/h.ft2.°F |
100°C | 13.8 W/m.°C | |
| 400°F |
109 Btu.in/h.ft2.°F |
200°C | 15.6 W/m.°C | |
| 600°F |
123 Btu.in/h.ft2.°F |
300°C | 17.5 W/m.°C | |
| 800°F |
138 Btu.in/h.ft2.°F |
400°C | 19.4 W/m.°C | |
| 1000°F |
155 Btu.in/h.ft2.°F |
500°C | 21.5 W/m.°C | |
| - | - | 600°C | 23.9 W/m.°C | |
| Thermal Diffusivity | RT |
0.005 in.2/s |
RT |
0.033 x 10-6cm2/s |
| 200°F |
0.005 in.2/s |
100°C |
0.035 x 10-6cm2/s |
|
| 400°F |
0.006 in.2/s |
200°C |
0.038 x 10-6cm2/s |
|
| 600°F |
0.007 in.2/s |
300°C |
0.042 x 10-6cm2/s |
|
| 800°F |
0.007 in.2/s |
400°C |
0.045 x 10-6cm2/s |
|
| 1000°F |
0.007 in.2/s |
500°C |
0.047 x 10-6cm2/s |
|
| - | - | 600°C |
0.050 x 10-6cm2/s |
|
| Mean Coefficient of Thermal Expansion | 78-200°F | 7.2 µin/in.°F | 26-100°C | 13.0 µm/m.°C |
| 78-400°F | 7.5 µin/in.°F | 26-200°C | 13.4 µm/m.°C | |
| 78-600°F | 7.8 µin/in.°F | 26-300°C | 14.0 µm/m.°C | |
| 78-800°F | 8.0 µin/in.°F | 26-400°C | 14.3 µm/m.°C | |
| 78-1000°F | 8.2 µin/in.°F | 26-500°C | 14.8 µm/m.°C | |
| 78-1200°F | 8.4 µin/in.°F | 26-600°C | 15.0 µm/m.°C | |
| 78-1400°F | 8.8 µin/in.°F | 26-700°C | 15.4 µm/m.°C | |
| 78-1600°F | 9.1 µin/in.°F | 26-800°C | 16.1 µm/m.°C | |
| Specific Heat | 100°F | 0.110 Btu/lb.°F | RT | 456 J/kg.°C |
| 200°F | 0.112 Btu/lb.°F | 100°C | 470 J/kg.°C | |
| 400°F | 0.116 Btu/lb.°F | 200°C | 482 J/kg.°C | |
| 600°F | 0.121 Btu/lb.°F | 300°C | 504 J/kg.°C | |
| 800°F | 0.127 Btu/lb.°F | 400°C | 525 J/kg.°C | |
| 1000°F | 0.133 Btu/lb.°F | 500°C | 545 J/kg.°C | |
| - | - | 600°C | 573 J/kg.°C | |
| Dynamic Modulus of Elasticity | RT |
33.2 X 106psi |
RT | 229 GPa |
| 200°F |
32.6 X 106psi |
100°C | 224 GPa | |
| 400°F |
31.2 X 106psi |
200°C | 216 GPa | |
| 600°F |
29.9 X 106psi |
300°C | 208 GPa | |
| 800°F |
28.6 X 106psi |
400°C | 199 GPa | |
| 1000°F |
27.4 X 106psi |
500°C | 192 GPa | |
| 1200°F |
26.1 X 106psi |
600°C | 184 GPa | |
| Melting Range | 2430-2470°F | - | 1332-1354°C | - |
RT= Room Temperature
Impact Strength
These impact strengths were generated using Charpy V-notch samples, machined from mill annealed plate of thickness 12.7 mm (0.5 in).
| Test Temperature | Impact Strength | ||
| °F | °C | ft-lbf | J |
| RT | RT | 130 | 176 |
| -40 | -40 | 125 | 169 |
| -80 | -62 | 119 | 161 |
| -320 | -196 | 68 | 92 |
RT= Room Temperature
Tensile Strength and Elongation
| Form | Test Temperature | Thickness/ Bar Diameter | 0.2% Offset Yield Strength | Ultimate Tensile Strength | Elongation | ||||
| °F | °C | in | mm | ksi | MPa | ksi | Mpa | % | |
| Sheet | RT | RT | 0.063 | 1.6 | 72 | 496 | 138 | 951 | 42 |
| Sheet | 200 | 93 | 0.063 | 1.6 | 58 | 400 | 135 | 931 | 50 |
| Sheet | 400 | 204 | 0.063 | 1.6 | 45 | 310 | 134 | 924 | 62 |
| Sheet | 600 | 316 | 0.063 | 1.6 | 43 | 296 | 130 | 896 | 75 |
| Sheet | 800 | 427 | 0.063 | 1.6 | 41 | 283 | 120 | 827 | 76 |
| Plate | RT | RT | 0.25-1.5 | 6.4-38.1 | 79 | 545 | 148 | 1020 | 36 |
| Plate | 200 | 93 | 0.25-1.5 | 6.4-38.1 | 70 | 483 | 143 | 986 | 40 |
| Plate | 400 | 204 | 0.25-1.5 | 6.4-38.1 | 55 | 379 | 143 | 986 | 61 |
| Plate | 600 | 316 | 0.25-1.5 | 6.4-38.1 | 48 | 331 | 138 | 951 | 70 |
| Plate | 800 | 427 | 0.25-1.5 | 6.4-38.1 | 45 | 310 | 133 | 917 | 70 |
| Plate | 1000 | 538 | 0.25-1.5 | 6.4-38.1 | 38 | 262 | 125 | 862 | 70 |
| Plate | 1200 | 649 | 0.25-1.5 | 6.4-38.1 | 37 | 255 | 99 | 683 | 66 |
| Plate | 1400 | 790 | 0.25-1.5 | 6.4-38.1 | 39 | 269 | 76 | 524 | 70 |
| Plate | 1600 | 871 | 0.25-1.5 | 6.4-38.1 | 28 | 193 | 51 | 352 | 77 |
| Plate | 1800 | 982 | 0.25-1.5 | 6.4-38.1 | 16 | 110 | 31 | 214 | 100 |
| Bar | RT | RT | 0.5-2.0 | 12.7-50.8 | 76 | 524 | 147 | 1014 | 38 |
| Bar | 200 | 93 | 0.5-2.0 | 12.7-50.8 | 70 | 483 | 140 | 965 | 49 |
| Bar | 400 | 204 | 0.5-2.0 | 12.7-50.8 | 52 | 359 | 140 | 965 | 66 |
| Bar | 600 | 316 | 0.5-2.0 | 12.7-50.8 | 44 | 303 | 132 | 910 | 77 |
| Bar | 800 | 427 | 0.5-2.0 | 12.7-50.8 | 43 | 296 | 131 | 903 | 84 |
| Bar | 1000 | 538 | 0.5-2.0 | 12.7-50.8 | 40 | 276 | 114 | 793 | 79 |
RT= Room Temperature
Hardness
In the annealed condition, ULTIMET alloy is not very hard. However, it has a high work-hardening rate, and even stretching of sheets and flattening of plates during mill processing can increase its hardness. The hardnesses in this table were measured on mill sheets, and indicate how rapidly the alloy hardens upon cold working.
| Condition | Hardness, HRC |
| Mill Annealed | 30 |
| 10% Cold-Work | 40 |
| 20% Cold-Worked | 43 |
| 40% Cold-Worked | 49 |
HRC = Hardness Rockwell “C”.
Welding and Fabrication
ULTIMET® alloy is very amenable to the Gas Metal Arc (GMA/MIG), Gas Tungsten Arc (GTA/TIG), and Shielded Metal Arc (SMA/Stick) welding processes. Matching filler metals (i.e. spools, reels, coils, and cut straight lengths of solid wire, and coated electrodes) are available for these processes. Guidelines for weld surfacing with ULTIMET® alloy are detailed in a separate Haynes International document “ULTIMET® Weld Overlay Guidelines“. Other arc processes have been used to weld ULTIMET® alloy; for more information on consumable availability for these other processes, please consult Haynes International.
Wrought products of ULTIMET® alloy are supplied in the Mill Annealed (MA) condition, unless otherwise specified. This solution annealing procedure has been designed to optimize the alloy’s corrosion resistance and ductility. Following all hot forming operations, the material should be re-annealed, to restore optimum properties. The alloy should also be re-annealed after any cold forming operations that result in an outer fiber elongation of 7% or more. The annealing temperature for ULTIMET® alloy is 1177°C (2150°F), and water quenching is advised (rapid air cooling is feasible with structures thinner than 10 mm (0.375 in). A hold time at the annealing temperature of 10 to 30 minutes is recommended, depending on the thickness of the structure (thicker structures need the full 30 minutes).
ULTIMET® alloy can be hot worked and cold-worked. However, it is very strong, and work-hardens rapidly during cold-working. The alloy may therefore require frequent, intermediate anneals, if cold-working is employed. Please consult Haynes International for more details.
While cold-work does not usually affect the resistance of ULTIMET® alloy to general corrosion, and to chloride-induced pitting and crevice attack, it can affect resistance to stress corrosion cracking. For optimum corrosion performance, therefore, the re-annealing of cold-worked parts (following an outer fiber elongation of 7% or more) is important.
Welding Data
Typical Transverse Tensile Data, Weldments
| Form | Weld Type | Test Temperature | 0.2% Offset Yield Strength | Ultimate Tensile Strength | Elongation | |
| - | - | °F | °C | ksi* | ksi* | % |
| Plate 1/2 in. (12.7mm) thick | GTAW | RT | RT | 89 | 127 | 11 |
| GMAW (Short) | RT | RT | 98 | 121 | 6 | |
| 500 | 260 | 65 | 121 | 19 | ||
| 1000 | 538 | 53 | 114 | 28 | ||
| GMAW (Spray) | RT | RT | 93 | 133 | 11 | |
| 500 | 260 | 67 | 121 | 19 | ||
| 1000 | 5.38 | 65 | 113 | 30 | ||
| SMAW | RT | RT | 97 | 135 | 9 | |
| Plate 3/4 (19.1mm) thick | GMAW (Short) | RT | RT | 86 | 123 | 10 |
| 500 | 260 | 62 | 116 | 20 | ||
| 1000 | 538 | 45 | 98 | 26 | ||
| GMAW (Spray) | RT | RT | 90 | 136 | 15 | |
| 500 | 260 | 64 | 121 | 23 | ||
| 1000 | 538 | 50 | 113 | 32 | ||
| SMAW | RT | RT | 87 | 130 | 13 | |
| 1000 | 538 | 48 | 109 | 32 | ||
*ksi can be converted to MPa (megapascals) by multiplying by 6.895.
Typical Tensile Data, All-Weld Metal
| Weld Type | Test Temperature | 0.2% Offset Yield Strength | Ultimate Tensile Strength | Elongation | |
| - | °F | °C | ksi* | ksi* | % |
| GTAW | RT | - | 95 | 133 | 10 |
| GMAW (Short) | RT | - | 89 | 132 | 17 |
| GMAW (Spray) | RT | - | 85 | 123 | 18 |
| SMAW | RT | - | 93 | 13 | 16 |
| 1000 | - | 61 | 100 | 31 | |
Typical Impact Strength, Weldments
| Weld Type | V-Notch Impact Strength Room Temperature | |
| - | ft.-lb. | J |
| GTAW | 94 | 127 |
| SMAW | 42 | 57 |
Typical Bend Test Data, Welded Plate
| Weld Type | Face Bend | Side Bend | ||
| - | 2T | 3T | 2T | 3T |
| GMAW (Short) | Failed | Passed | Failed | Passed |
| GMAW (Spray) | Failed | Passed | Failed | Passed |
| SMAW | - | Passed | - | - |
Duplicate specimens, 3/4 in. (19.10 mm) thick. Tested using AWS Specification 5.11 as a guide.
Specifications and Codes
Specifications
| ULTIMET® (R31233) | |
| Sheet, Plate & Strip | SB818/B818 |
| Billet, Rod & Bar | B815 |
| Coated Electrodes | - |
| Bare Welding Rods & Wire | SFA / A5.21 (ERCoCr-H) |
| Seamless Pipe & Tube | - |
| Welded Pipe & Tube | - |
| Fittings | - |
| Forgings | - |
| DIN | No. 2.4681CoCr26Ni9Mo5W |
| TÜV | - |
| Others | NACE MR0175/MR0103ISO 15156 |
Codes
| ULTIMET® (R31233) | |||
| ASME | Section l | - | |
| Section lll | Class 1 | - | |
| Class 2 | - | ||
| Class 3 | - | ||
| Section Vlll | Div. 1 | 800°F (427°C) | |
| Div. 2 | - | ||
| Section Xll | - | ||
| B16.5 | - | ||
| B16.34 | - | ||
| B31.1 | - | ||
| B31.3 | - | ||
| VdTÜV (doc #) | - | ||
1Plate, Sheet, Bar
Disclaimer
Haynes International makes all reasonable efforts to ensure the accuracy and correctness of the data displayed on this site but makes no representations or warranties as to the data’s accuracy, correctness or reliability. All data are for general information only and not for providing design advice. Alloy properties disclosed here are based on work conducted principally by Haynes International, Inc. and occasionally supplemented by information from the open literature and, as such, are indicative only of the results of such tests and should not be considered guaranteed maximums or minimums. It is the responsibility of the user to test specific alloys under actual service conditions to determine their suitability for a particular purpose.
For specific concentrations of elements present in a particular product and a discussion of the potential health affects thereof, refer to the Safety Data Sheets supplied by Haynes International, Inc. All trademarks are owned by Haynes International, Inc., unless otherwise indicated.