{"id":13067,"date":"2024-08-06T16:16:31","date_gmt":"2024-08-06T16:16:31","guid":{"rendered":"https:\/\/haynesintl.com\/alloys\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\/haynes-188\/"},"modified":"2025-02-24T13:51:36","modified_gmt":"2025-02-24T13:51:36","slug":"haynes-188-%e5%90%88%e9%87%91","status":"publish","type":"alloys","link":"https:\/\/haynesintl.com\/zh-hans\/alloys\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\/haynes-188-%e5%90%88%e9%87%91\/","title":{"rendered":"HAYNES<sup>\u00ae<\/sup> 188 \u5408\u91d1"},"content":{"rendered":"\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-principal-features\">Principal Features<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HAYNES<sup>\u00ae<\/sup> 188 alloy (UNS R30188) is a cobalt-nickel-chromium-tungsten alloy that combines excellent high-temperature strength with very good resistance to oxidizing environments up to 2000\u00b0F (1095\u00b0C) for prolonged exposures, and excellent resistance to sulfate deposit hot corrosion. It is readily fabricated and formed by conventional techniques, and has been used for cast component. Other attractive features include excellent resistance to molten chloride salts, and good resistance to gaseous sulfidation.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-readily-fabricated\">Readily Fabricated<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">HAYNES<sup>\u00ae<\/sup> 188 alloy has good forming and welding characteristics. It may be forged or other hot-worked, providing that it is held at 2150\u00b0F (1175\u00b0C) for a time sufficient to bring the entire piece to temperature. As a consequence of its good ductility, 188 alloy is also readily formed by cold working. The alloy does work-harden rapidly, however, so frequent intermediate annealing treatments may be needed for complex component forming operations. All hot- or cold- worked parts should be annealed and rapidly cooled in order to restore the best balance of properties.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The alloy can be welded by both manual and automatic welding methods, including gas tungsten arc (TIG), gas metal arc (MIG), electron beam and resistance welding. It exhibits good restraint welding characteristics.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-heat-treatment\">Heat Treatment<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Wrought HAYNES<sup>\u00ae<\/sup> 188 alloy is furnished in the solution heat treated condition, unless otherwise specified. The alloy is normally solution heat-treated at 2125-2175\u00b0F (1163-1191\u00b0C) and rapidly cooled or water quenched for optimal properties.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Annealing at temperatures less than the solution heat-treating temperature will produce some carbide precipitation in alloy 188, which may affect the alloy\u2019s properties.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-applications\">Applications<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">HAYNES<sup>\u00ae<\/sup> 188 alloy combines properties which make is suitable for a variety of fabricated component applications in the aerospace industry. It is widely used in established military and commercial gas turbine engines for combustion cans, transitions ducts, and afterburner components. It shares applications in newer engine programs with a more recently developed material, 230<sup>\u00ae<\/sup> alloy, which possesses improved properties.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">*Please contact our <a href=\"https:\/\/haynesintl.com\/zh-hans\/%e9%94%80%e5%94%ae%e4%ba%ba%e5%91%98\/%e6%8a%80%e6%9c%af%e6%94%af%e6%8c%81\/\" target=\"_blank\" rel=\"noopener\">technical support team<\/a> if you have technical questions about this alloy.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-nominal-composition\">Nominal Composition<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-58\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"2\"\n           data-rows=\"11\"\n           data-wpID=\"58\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        Weight %                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Cobalt                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        39 Balance                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Nickel                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Chromium                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Tungsten                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Iron                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Manganese                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.25 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Silicon                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.35                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Carbon                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Lanthanum                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Boron                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.015 max.                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-58'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-creep-and-stress-rupture-strength\">Creep and Stress-Rupture Strength<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HAYNES 188 alloy is a solid-solution- strengthened material which combines excellent high-temperature strength with good fabricability at room temperature. It is particularly effective for very long-term applications at temperatures of 1200\u00b0F (650\u00b0C) or more. It is stronger than nickel-base solid-solution-strengthened alloys, and far stronger than simple nickel chromium or iron-nickel-chromium heat-resistant alloys. This can allow for significant section thickness reduction when it is substituted for these materials.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-comparision-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours\">Comparision of Sheet Materials: Stress to Produce 1% Creep in 1000 Hours<\/h3>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"704\" height=\"396\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparison-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours.png?resize=704%2C396&#038;ssl=1\" alt=\"\" class=\"wp-image-2152\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparison-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours.png?w=704&amp;ssl=1 704w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparison-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours.png?resize=300%2C169&amp;ssl=1 300w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparison-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours.png?resize=620%2C349&amp;ssl=1 620w\" sizes=\"(max-width: 704px) 100vw, 704px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-188-plate-solution-annealed\">188 Plate, Solution-Annealed<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-43\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"11\"\n           data-rows=\"30\"\n           data-wpID=\"43\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:18.181818181818%;                    padding:10px;\n                    \"\n                    >\n                                        Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:9.0909090909091%;                    padding:10px;\n                    \"\n                    >\n                                        Creep                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"8\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:72.727272727273%;                    padding:10px;\n                    \"\n                    >\n                                        Approximate Initial Stress to Produce Specified Creep in                    <\/td>\n                                                                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10 h                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100 h                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1,000 h                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"J2\"\n                    data-col-index=\"9\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10,000 h                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"K3\"\n                    data-col-index=\"10\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K4\"\n                    data-col-index=\"10\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        35*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        241*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K5\"\n                    data-col-index=\"10\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        78                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        59                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        407                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K6\"\n                    data-col-index=\"10\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        310*                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1300                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        704                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        41                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        283                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        193                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        124*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K7\"\n                    data-col-index=\"10\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        303                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        31.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        217                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        152                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K8\"\n                    data-col-index=\"10\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        73*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        503*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        372                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        276                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K9\"\n                    data-col-index=\"10\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        193                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        179                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        117                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K10\"\n                    data-col-index=\"10\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        141                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14.5*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K11\"\n                    data-col-index=\"10\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        51                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        352                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        37                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        255                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        179                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J12\"\n                    data-col-index=\"9\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18.5*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K12\"\n                    data-col-index=\"10\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        128*                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1500                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        816                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        110                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        76                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.7*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I13\"\n                    data-col-index=\"8\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        53*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J13\"\n                    data-col-index=\"9\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K13\"\n                    data-col-index=\"10\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        131                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I14\"\n                    data-col-index=\"8\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        64                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J14\"\n                    data-col-index=\"9\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K14\"\n                    data-col-index=\"10\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        36                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        248                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        172                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I15\"\n                    data-col-index=\"8\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        121                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J15\"\n                    data-col-index=\"9\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K15\"\n                    data-col-index=\"10\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        83                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.5*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I16\"\n                    data-col-index=\"8\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J16\"\n                    data-col-index=\"9\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K16\"\n                    data-col-index=\"10\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        90                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H17\"\n                    data-col-index=\"7\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.4*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I17\"\n                    data-col-index=\"8\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J17\"\n                    data-col-index=\"9\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K17\"\n                    data-col-index=\"10\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        172                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F18\"\n                    data-col-index=\"5\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G18\"\n                    data-col-index=\"6\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        117                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H18\"\n                    data-col-index=\"7\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I18\"\n                    data-col-index=\"8\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J18\"\n                    data-col-index=\"9\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K18\"\n                    data-col-index=\"10\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A19\"\n                    data-col-index=\"0\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1700                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B19\"\n                    data-col-index=\"1\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        927                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C19\"\n                    data-col-index=\"2\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F19\"\n                    data-col-index=\"5\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G19\"\n                    data-col-index=\"6\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        36                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H19\"\n                    data-col-index=\"7\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.6*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I19\"\n                    data-col-index=\"8\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J19\"\n                    data-col-index=\"9\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K19\"\n                    data-col-index=\"10\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F20\"\n                    data-col-index=\"5\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G20\"\n                    data-col-index=\"6\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        41                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H20\"\n                    data-col-index=\"7\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.3*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I20\"\n                    data-col-index=\"8\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J20\"\n                    data-col-index=\"9\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K20\"\n                    data-col-index=\"10\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C21\"\n                    data-col-index=\"2\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D21\"\n                    data-col-index=\"3\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E21\"\n                    data-col-index=\"4\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        114                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F21\"\n                    data-col-index=\"5\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G21\"\n                    data-col-index=\"6\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H21\"\n                    data-col-index=\"7\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I21\"\n                    data-col-index=\"8\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J21\"\n                    data-col-index=\"9\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.5*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K21\"\n                    data-col-index=\"10\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        31*                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A22\"\n                    data-col-index=\"0\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B22\"\n                    data-col-index=\"1\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        982                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C22\"\n                    data-col-index=\"2\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D22\"\n                    data-col-index=\"3\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E22\"\n                    data-col-index=\"4\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        39                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F22\"\n                    data-col-index=\"5\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G22\"\n                    data-col-index=\"6\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H22\"\n                    data-col-index=\"7\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I22\"\n                    data-col-index=\"8\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J22\"\n                    data-col-index=\"9\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.35                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K22\"\n                    data-col-index=\"10\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.3                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C23\"\n                    data-col-index=\"2\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D23\"\n                    data-col-index=\"3\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E23\"\n                    data-col-index=\"4\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F23\"\n                    data-col-index=\"5\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G23\"\n                    data-col-index=\"6\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H23\"\n                    data-col-index=\"7\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I23\"\n                    data-col-index=\"8\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J23\"\n                    data-col-index=\"9\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.42                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K23\"\n                    data-col-index=\"10\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.8                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C24\"\n                    data-col-index=\"2\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D24\"\n                    data-col-index=\"3\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E24\"\n                    data-col-index=\"4\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F24\"\n                    data-col-index=\"5\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G24\"\n                    data-col-index=\"6\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        48                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H24\"\n                    data-col-index=\"7\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I24\"\n                    data-col-index=\"8\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J24\"\n                    data-col-index=\"9\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.2*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K24\"\n                    data-col-index=\"10\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15*                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A25\"\n                    data-col-index=\"0\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1900                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B25\"\n                    data-col-index=\"1\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1038                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C25\"\n                    data-col-index=\"2\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D25\"\n                    data-col-index=\"3\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E25\"\n                    data-col-index=\"4\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F25\"\n                    data-col-index=\"5\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.3*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G25\"\n                    data-col-index=\"6\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H25\"\n                    data-col-index=\"7\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I25\"\n                    data-col-index=\"8\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J25\"\n                    data-col-index=\"9\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K25\"\n                    data-col-index=\"10\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C26\"\n                    data-col-index=\"2\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D26\"\n                    data-col-index=\"3\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E26\"\n                    data-col-index=\"4\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F26\"\n                    data-col-index=\"5\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.5*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G26\"\n                    data-col-index=\"6\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H26\"\n                    data-col-index=\"7\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I26\"\n                    data-col-index=\"8\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J26\"\n                    data-col-index=\"9\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K26\"\n                    data-col-index=\"10\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C27\"\n                    data-col-index=\"2\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D27\"\n                    data-col-index=\"3\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.2*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E27\"\n                    data-col-index=\"4\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F27\"\n                    data-col-index=\"5\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G27\"\n                    data-col-index=\"6\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H27\"\n                    data-col-index=\"7\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.2*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I27\"\n                    data-col-index=\"8\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J27\"\n                    data-col-index=\"9\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K27\"\n                    data-col-index=\"10\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A28\"\n                    data-col-index=\"0\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B28\"\n                    data-col-index=\"1\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1093                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C28\"\n                    data-col-index=\"2\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D28\"\n                    data-col-index=\"3\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E28\"\n                    data-col-index=\"4\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F28\"\n                    data-col-index=\"5\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.35                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G28\"\n                    data-col-index=\"6\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H28\"\n                    data-col-index=\"7\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I28\"\n                    data-col-index=\"8\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J28\"\n                    data-col-index=\"9\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K28\"\n                    data-col-index=\"10\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C29\"\n                    data-col-index=\"2\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D29\"\n                    data-col-index=\"3\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E29\"\n                    data-col-index=\"4\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F29\"\n                    data-col-index=\"5\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.42                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G29\"\n                    data-col-index=\"6\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H29\"\n                    data-col-index=\"7\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I29\"\n                    data-col-index=\"8\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J29\"\n                    data-col-index=\"9\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K29\"\n                    data-col-index=\"10\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C30\"\n                    data-col-index=\"2\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D30\"\n                    data-col-index=\"3\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E30\"\n                    data-col-index=\"4\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        32                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F30\"\n                    data-col-index=\"5\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G30\"\n                    data-col-index=\"6\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H30\"\n                    data-col-index=\"7\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.10*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I30\"\n                    data-col-index=\"8\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.6*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J30\"\n                    data-col-index=\"9\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K30\"\n                    data-col-index=\"10\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2014                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-43'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Significant extrapolation<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-188-sheet-solution-annealed\">188 Sheet, Solution-Annealed<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-44\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"9\"\n           data-rows=\"24\"\n           data-wpID=\"44\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:22.222222222222%;                    padding:10px;\n                    \"\n                    >\n                                        Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:11.111111111111%;                    padding:10px;\n                    \"\n                    >\n                                        Creep                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"6\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:66.666666666667%;                    padding:10px;\n                    \"\n                    >\n                                        Approximate Initial Stress to Produce Specified Creep in                    <\/td>\n                                                                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10 h                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100 h                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1,000 h                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        155                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        113                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        81                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        176                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        128                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        92                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43.0*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        296*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        32.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        221                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        23.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        159                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1500                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        816                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        121                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        87                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        31.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        214                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        150                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        103                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        74                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        34                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        84                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        58                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        39                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        145                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        99                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1700                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        927                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        34                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I13\"\n                    data-col-index=\"8\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        57                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        39                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I14\"\n                    data-col-index=\"8\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        99                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.5*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I15\"\n                    data-col-index=\"8\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38*                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        982                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        34                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I16\"\n                    data-col-index=\"8\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        39                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H17\"\n                    data-col-index=\"7\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I17\"\n                    data-col-index=\"8\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F18\"\n                    data-col-index=\"5\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G18\"\n                    data-col-index=\"6\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        37                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H18\"\n                    data-col-index=\"7\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I18\"\n                    data-col-index=\"8\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A19\"\n                    data-col-index=\"0\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1900                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B19\"\n                    data-col-index=\"1\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1038                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C19\"\n                    data-col-index=\"2\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F19\"\n                    data-col-index=\"5\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G19\"\n                    data-col-index=\"6\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H19\"\n                    data-col-index=\"7\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I19\"\n                    data-col-index=\"8\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.3                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F20\"\n                    data-col-index=\"5\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G20\"\n                    data-col-index=\"6\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H20\"\n                    data-col-index=\"7\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I20\"\n                    data-col-index=\"8\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.7                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C21\"\n                    data-col-index=\"2\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D21\"\n                    data-col-index=\"3\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E21\"\n                    data-col-index=\"4\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F21\"\n                    data-col-index=\"5\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G21\"\n                    data-col-index=\"6\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H21\"\n                    data-col-index=\"7\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I21\"\n                    data-col-index=\"8\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A22\"\n                    data-col-index=\"0\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B22\"\n                    data-col-index=\"1\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1093                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C22\"\n                    data-col-index=\"2\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D22\"\n                    data-col-index=\"3\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.0*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E22\"\n                    data-col-index=\"4\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F22\"\n                    data-col-index=\"5\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G22\"\n                    data-col-index=\"6\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H22\"\n                    data-col-index=\"7\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I22\"\n                    data-col-index=\"8\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.8                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C23\"\n                    data-col-index=\"2\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D23\"\n                    data-col-index=\"3\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.3*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E23\"\n                    data-col-index=\"4\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F23\"\n                    data-col-index=\"5\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G23\"\n                    data-col-index=\"6\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H23\"\n                    data-col-index=\"7\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.90                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I23\"\n                    data-col-index=\"8\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.2                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C24\"\n                    data-col-index=\"2\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D24\"\n                    data-col-index=\"3\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.3*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E24\"\n                    data-col-index=\"4\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        23*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F24\"\n                    data-col-index=\"5\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G24\"\n                    data-col-index=\"6\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H24\"\n                    data-col-index=\"7\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I24\"\n                    data-col-index=\"8\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.3                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-44'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Significant extrapolation<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-tensile-properties\">Tensile Properties<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-hot-rolled-and-solution-annealed-plate\">Hot-Rolled and Solution-annealed Plate<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-84\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"7\"\n           data-rows=\"9\"\n           data-wpID=\"84\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:28.571428571429%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:28.571428571429%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:28.571428571429%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate Tensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:14.285714285714%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70.1                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        483                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        143.8                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        991                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50.6                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45.7                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        315                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        120.6                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        832                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60.3                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45.1                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        311                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        121.6                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        838                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62.8                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43.6                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        301                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        84.1                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        580                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        85.6                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        37.1                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        256                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.5                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        341                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        97.9                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        982                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19.2                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        132                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        27.2                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        188                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        102.6                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1093                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.6                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.9                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        96                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444\"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        87.1                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-84'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-cold-rolled-and-solution-annealed-sheet\">Cold-Rolled and Solution-annealed Sheet<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-86\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"7\"\n           data-rows=\"9\"\n           data-wpID=\"86\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:28.571428571429%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:28.571428571429%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:28.571428571429%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate\nTensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:14.285714285714%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        483                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        142.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        982                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50.9                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        309                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        117.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        809                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        58.8                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        309                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        119.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        821                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        58.6                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        302                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        81.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        563                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        81.8                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        37.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        261                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        324                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        103.9                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        982                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        125                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        175                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        81.0                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1093                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        59                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        85                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.7                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-86'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-hardness-data\">Hardness Data<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-solution-annealed-room-temperature-hardness\">Solution Annealed Room Temperature Hardness<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-54\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"3\"\n           data-rows=\"4\"\n           data-wpID=\"54\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:33.333333333333%;                    padding:10px;\n                    \"\n                    >\n                                        Form                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:33.333333333333%;                    padding:10px;\n                    \"\n                    >\n                                        Hardness, HRBW                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:33.333333333333%;                    padding:10px;\n                    \"\n                    >\n                                        Typical ASTM Grain Size                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        98                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5 \u2013 7.5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        98                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4 \u2013 8                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Bar                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        96                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.5 \u2013 7.5                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-54'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-FFFFFF { background-color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">All samples tested in solution-annealed condition<br>HRBW = Hardness Rockwell \u201cB\u201d, Tungsten Indentor.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-high-temperature-hardness\">High-Temperature Hardness<\/h2>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"600\" height=\"362\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188hardness.tmb-ze-600-600.png?resize=600%2C362&#038;ssl=1\" alt=\"\" class=\"wp-image-2156\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188hardness.tmb-ze-600-600.png?w=600&amp;ssl=1 600w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188hardness.tmb-ze-600-600.png?resize=300%2C181&amp;ssl=1 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/figure>\n<\/div>\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n wdtscroll\"\n    >\n        <table id=\"wpdtSimpleTable-55\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"12\"\n           data-rows=\"10\"\n           data-wpID=\"55\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:106px;                    padding:10px;\n                    \"\n                    >\n                                        Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:162px;                    padding:10px;\n                    \"\n                    >\n                                        188                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:172px;                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:172px;                    padding:10px;\n                    \"\n                    >\n                                        6B                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:176px;                    padding:10px;\n                    \"\n                    >\n                                        230<sup>\u00ae<\/sup>                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"K1\"\n                    data-col-index=\"10\"\n                    data-row-index=\"0\"\n                    style=\" width:168px;                    padding:10px;\n                    \"\n                    >\n                                        556<sup>\u00ae<\/sup>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Vickers Hardness                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Rockwell Hardness                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Vickers Hardness                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Rockwell Hardness                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Vickers Hardness                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Rockwell Hardness                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Vickers Hardness                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"J2\"\n                    data-col-index=\"9\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Rockwell Hardness                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"K2\"\n                    data-col-index=\"10\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Vickers Hardness                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"L2\"\n                    data-col-index=\"11\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Rockwell Hardness                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        DPN                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HR C\/BW                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        DPN                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HR C\/BW                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        DPN                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HR C\/BW                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        DPN                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HR C\/B                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"K3\"\n                    data-col-index=\"10\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        DPN                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"L3\"\n                    data-col-index=\"11\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HR C\/BW                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        72                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        248                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21.8 C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        285                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        27.8 C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        374                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38.2 C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        195                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        92.0 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K4\"\n                    data-col-index=\"10\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        203                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L4\"\n                    data-col-index=\"11\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93.6 BW                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        427                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        170                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        86.3 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        171                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        86.7 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        269                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25.5 C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        142                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77.3 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K5\"\n                    data-col-index=\"10\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        132                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L5\"\n                    data-col-index=\"11\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        73.0 BW                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        159                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        83.0 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        160                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        73.3 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        247                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21.8 C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        139                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        76.0 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K6\"\n                    data-col-index=\"10\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        129                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L6\"\n                    data-col-index=\"11\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        71.1 BW                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        147                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77.2 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        150                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80.0 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        225                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        97.5 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        132                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        73.0 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K7\"\n                    data-col-index=\"10\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        118                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L7\"\n                    data-col-index=\"11\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66.5 BW                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        129                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70.7 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        134                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        73.7 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        153                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        81.0 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        125                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70.0 BW                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K8\"\n                    data-col-index=\"10\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L8\"\n                    data-col-index=\"11\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55.0 BW                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        89                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        91                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K9\"\n                    data-col-index=\"10\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        67                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L9\"\n                    data-col-index=\"11\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        982                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        42                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K10\"\n                    data-col-index=\"10\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        41*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L10\"\n                    data-col-index=\"11\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-55'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">HRC = Hardness Rockwell \u201cC\u201d.<br>HRBW = Hardness Rockwell \u201cB\u201d, Tungsten Indentor.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-impact-strength-properties\">Impact Strength Properties<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-57\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"4\"\n           data-rows=\"7\"\n           data-wpID=\"57\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:50%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:50%;                    padding:10px;\n                    \"\n                    >\n                                        Typical Charpy V-Notch Impact Resistance                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ft.-lbs                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        J                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -300                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -185                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        116                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        158                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -150                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -100                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        131                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        178                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        143                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        194                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        540                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        117                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        159                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1300                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        705                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        145                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-57'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Average of longitudinal and transverse tests on solution-annealed plate<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-thermal-stability\">Thermal Stability<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HAYNES<sup>\u00ae<\/sup> 188 alloy is similar to the solid-solution-strengthened superalloys, such as alloy 625 or HASTELLOY<sup>\u00ae<\/sup> X alloy,  which will precipitate deleterious phases upon such long-term exposure. In this case. the phase in question is a CO<sub>2<\/sub>W laves phase.  which serves to impair both tensile ductility and impact strength. The behavior of 188 alloy is significantly better in this regard than HAYNES<sup>\u00ae<\/sup> 25 alloy, which it replaced; but for applications where thermal stability is important, 230<sup>\u00ae<\/sup> alloy is recommended.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"500\" height=\"451\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-alloy-thermalex_c60422c8-7d17-494b-8475-404356059fe5.tmb-ze-500-500.png?resize=500%2C451&#038;ssl=1\" alt=\"\" class=\"wp-image-2160\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-alloy-thermalex_c60422c8-7d17-494b-8475-404356059fe5.tmb-ze-500-500.png?w=500&amp;ssl=1 500w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-alloy-thermalex_c60422c8-7d17-494b-8475-404356059fe5.tmb-ze-500-500.png?resize=300%2C271&amp;ssl=1 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-room-temperature-properties-of-plate-after-thermal-exposure\">Room-Temperature Properties of Plate after Thermal Exposure<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-74\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"10\"\n           data-rows=\"11\"\n           data-wpID=\"74\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Exposure Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate Tensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Impact Strength                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        h                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ft.- lbs.                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"J2\"\n                    data-col-index=\"9\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        J                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        650                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        450                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        140.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        965                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        143                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        194                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        550                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        151.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1045                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        29.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        23                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        31                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        450                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        140.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        965                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        143                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        194                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        74.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        510                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        147.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1020                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"5\"                     data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"5\"                     data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        870                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        485                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        146.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1005                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        143                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        194                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        490                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        157.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1085                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        68.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        475                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        156.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1075                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        64.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        445                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        147.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1015                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        440                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        146.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1005                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-74'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Average of two test exposure. All other single exposures.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-comparative-impact-strength-after-8000-hour-exposures\">Comparative Impact Strength after 8000-Hour Exposures<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-76\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"9\"\n           data-rows=\"7\"\n           data-wpID=\"76\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:11.111111111111%;                    padding:10px;\n                    \"\n                    >\n                                        Alloy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"2\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:22.222222222222%;                    padding:10px;\n                    \"\n                    >\n                                        Solution-Annealed Charpy\nV-Notch Impact                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"6\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:66.666666666667%;                    padding:10px;\n                    \"\n                    >\n                                        Charpy V-Notch Impact Following Exposure\nFor 8000 Hours at Temperatures                    <\/td>\n                                                                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        650\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        870\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ft.-lbs.                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        J                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ft.-lbs                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        J                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ft.-lbs                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        J                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ft.-lbs                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        J                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        230<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        73                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        41                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        188                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        143                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        194                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        23                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        31                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        X                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        73                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        81                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        110                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-76'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n.wpdt-bc-FFFFFF { background-color: #FFFFFF !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-physical-properties\">Physical Properties<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-80\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"5\"\n           data-rows=\"90\"\n           data-wpID=\"80\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Physical Property                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Customary Units                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Metric Units                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Density                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">0.324 lb\/in<sup>3<\/sup><\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\"><p>8.98 g\/cm<sup>3<\/sup><\/p><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Melting Temperature                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2400-2570\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1315-1410\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"11\"                     data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Electrical Resistivity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        39.6 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        101.0 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40.3 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        103.0 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        41.5 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        105.0 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        42.7 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107.7 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43.8 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        110.5 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44.7 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        112.7 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45.6 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        114.8 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46.1 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        700\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        116.4 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46.5 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        117.5 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46.7 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        118.3 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46.8 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        119.1 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"11\"                     data-cell-id=\"A15\"\n                    data-col-index=\"0\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Specific Heat                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.096 Btu\/lb-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.1 J\/kg\u00b7\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.101 Btu\/lb-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        423 J\/kg\u00b7\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.106 Btu\/lb-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        444 J\/kg\u00b7\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B18\"\n                    data-col-index=\"1\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.112 Btu\/lb-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        465 J\/kg\u00b7\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B19\"\n                    data-col-index=\"1\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C19\"\n                    data-col-index=\"2\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.117 Btu\/lb-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        486 J\/kg\u00b7\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B20\"\n                    data-col-index=\"1\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.122 Btu\/lb-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        502 J\/kg\u00b7\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B21\"\n                    data-col-index=\"1\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C21\"\n                    data-col-index=\"2\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.127 Btu\/lb-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D21\"\n                    data-col-index=\"3\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E21\"\n                    data-col-index=\"4\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        523 J\/kg\u00b7\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B22\"\n                    data-col-index=\"1\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C22\"\n                    data-col-index=\"2\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.131 Btu\/lb-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D22\"\n                    data-col-index=\"3\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        700\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E22\"\n                    data-col-index=\"4\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        540 J\/kg\u00b7\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B23\"\n                    data-col-index=\"1\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C23\"\n                    data-col-index=\"2\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.136 Btu\/lb-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D23\"\n                    data-col-index=\"3\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E23\"\n                    data-col-index=\"4\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        557 J\/kg\u00b7\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B24\"\n                    data-col-index=\"1\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C24\"\n                    data-col-index=\"2\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.140 Btu\/lb-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D24\"\n                    data-col-index=\"3\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E24\"\n                    data-col-index=\"4\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        573 J\/kg\u00b7\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B25\"\n                    data-col-index=\"1\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000\u00b0 F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C25\"\n                    data-col-index=\"2\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.145 Btu\/lb-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D25\"\n                    data-col-index=\"3\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E25\"\n                    data-col-index=\"4\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        590 J\/kg\u00b7\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"11\"                     data-cell-id=\"A26\"\n                    data-col-index=\"0\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Thermal Conductivity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B26\"\n                    data-col-index=\"1\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C26\"\n                    data-col-index=\"2\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">72 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D26\"\n                    data-col-index=\"3\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E26\"\n                    data-col-index=\"4\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.4 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B27\"\n                    data-col-index=\"1\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C27\"\n                    data-col-index=\"2\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">84 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D27\"\n                    data-col-index=\"3\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E27\"\n                    data-col-index=\"4\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.2 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B28\"\n                    data-col-index=\"1\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C28\"\n                    data-col-index=\"2\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">100 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D28\"\n                    data-col-index=\"3\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E28\"\n                    data-col-index=\"4\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14.3 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B29\"\n                    data-col-index=\"1\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C29\"\n                    data-col-index=\"2\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">112 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D29\"\n                    data-col-index=\"3\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E29\"\n                    data-col-index=\"4\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15.9 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B30\"\n                    data-col-index=\"1\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C30\"\n                    data-col-index=\"2\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">125 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D30\"\n                    data-col-index=\"3\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E30\"\n                    data-col-index=\"4\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17.5 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B31\"\n                    data-col-index=\"1\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C31\"\n                    data-col-index=\"2\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">138 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D31\"\n                    data-col-index=\"3\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E31\"\n                    data-col-index=\"4\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19.3 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B32\"\n                    data-col-index=\"1\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C32\"\n                    data-col-index=\"2\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">152 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D32\"\n                    data-col-index=\"3\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E32\"\n                    data-col-index=\"4\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21.1 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B33\"\n                    data-col-index=\"1\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C33\"\n                    data-col-index=\"2\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">167 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D33\"\n                    data-col-index=\"3\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        700\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E33\"\n                    data-col-index=\"4\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        23.0 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B34\"\n                    data-col-index=\"1\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C34\"\n                    data-col-index=\"2\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">174 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D34\"\n                    data-col-index=\"3\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E34\"\n                    data-col-index=\"4\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24.8 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B35\"\n                    data-col-index=\"1\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C35\"\n                    data-col-index=\"2\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">189 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D35\"\n                    data-col-index=\"3\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E35\"\n                    data-col-index=\"4\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25.5 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B36\"\n                    data-col-index=\"1\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C36\"\n                    data-col-index=\"2\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">204 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D36\"\n                    data-col-index=\"3\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E36\"\n                    data-col-index=\"4\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        27.6 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"11\"                     data-cell-id=\"A37\"\n                    data-col-index=\"0\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Thermal Diffusivity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B37\"\n                    data-col-index=\"1\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C37\"\n                    data-col-index=\"2\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">4.5 x 10<sup>-3<\/sup> in<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D37\"\n                    data-col-index=\"3\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E37\"\n                    data-col-index=\"4\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">29.2 x 10<sup>-3<\/sup> cm<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B38\"\n                    data-col-index=\"1\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C38\"\n                    data-col-index=\"2\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">5.0 x 10<sup>-3<\/sup> in<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D38\"\n                    data-col-index=\"3\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E38\"\n                    data-col-index=\"4\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">32.7 x 10<sup>-3<\/sup> cm<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B39\"\n                    data-col-index=\"1\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C39\"\n                    data-col-index=\"2\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">5.6 x 10<sup>-3<\/sup> in<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D39\"\n                    data-col-index=\"3\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E39\"\n                    data-col-index=\"4\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">36.5 x 10<sup>-3<\/sup> cm<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B40\"\n                    data-col-index=\"1\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C40\"\n                    data-col-index=\"2\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">6.0 x 10<sup>-3<\/sup> in<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D40\"\n                    data-col-index=\"3\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E40\"\n                    data-col-index=\"4\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">38.7 x 10<sup>-3<\/sup> cm<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B41\"\n                    data-col-index=\"1\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C41\"\n                    data-col-index=\"2\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">6.4 x 10<sup>-3<\/sup> in<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D41\"\n                    data-col-index=\"3\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E41\"\n                    data-col-index=\"4\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">40.8 x 10<sup>-3<\/sup> cm<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B42\"\n                    data-col-index=\"1\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C42\"\n                    data-col-index=\"2\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">6.7 x 10<sup>-3<\/sup> \n in<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D42\"\n                    data-col-index=\"3\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E42\"\n                    data-col-index=\"4\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">43.5 x 10<sup>-3<\/sup> cm<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B43\"\n                    data-col-index=\"1\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C43\"\n                    data-col-index=\"2\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">7.1 x 10<sup>-3<\/sup> in<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D43\"\n                    data-col-index=\"3\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E43\"\n                    data-col-index=\"4\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">45.7 x 10<sup>-3<\/sup> cm<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B44\"\n                    data-col-index=\"1\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C44\"\n                    data-col-index=\"2\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">7.6 x 10<sup>-3<\/sup> in<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D44\"\n                    data-col-index=\"3\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        700\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E44\"\n                    data-col-index=\"4\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">48.2 x 10<sup>-3<\/sup> cm<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B45\"\n                    data-col-index=\"1\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C45\"\n                    data-col-index=\"2\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">7.6 x 10<sup>-3<\/sup> in<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D45\"\n                    data-col-index=\"3\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E45\"\n                    data-col-index=\"4\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">50.4 x 10<sup>-3<\/sup> cm<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B46\"\n                    data-col-index=\"1\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C46\"\n                    data-col-index=\"2\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">8.0 x 10<sup>-3<\/sup> in<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D46\"\n                    data-col-index=\"3\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E46\"\n                    data-col-index=\"4\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">50.4 x 10<sup>-3<\/sup> cm<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B47\"\n                    data-col-index=\"1\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C47\"\n                    data-col-index=\"2\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">8.4 x 10<sup>-3 <\/sup>in<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D47\"\n                    data-col-index=\"3\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E47\"\n                    data-col-index=\"4\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">53.0 x 10<sup>-3<\/sup> cm<sup>2<\/sup>\/sec<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"10\"                     data-cell-id=\"A48\"\n                    data-col-index=\"0\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Mean Coefficient of\nThermal Expansion                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B48\"\n                    data-col-index=\"1\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75 - 200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C48\"\n                    data-col-index=\"2\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">6.7 10<sup>-6<\/sup> in\/in\/&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D48\"\n                    data-col-index=\"3\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25 - 100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E48\"\n                    data-col-index=\"4\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">12.1 10<sup>-6<\/sup> m\/m\/&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B49\"\n                    data-col-index=\"1\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75 - 400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C49\"\n                    data-col-index=\"2\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">7.1 10<sup>-6<\/sup> in\/in\/&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D49\"\n                    data-col-index=\"3\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25 - 200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E49\"\n                    data-col-index=\"4\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">12.7 10<sup>-6<\/sup> m\/m\/&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B50\"\n                    data-col-index=\"1\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75 - 600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C50\"\n                    data-col-index=\"2\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">7.3 10<sup>-6<\/sup> in\/in\/&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D50\"\n                    data-col-index=\"3\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25 - 300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E50\"\n                    data-col-index=\"4\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">13.1 10<sup>-6<\/sup> m\/m\/&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B51\"\n                    data-col-index=\"1\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75 - 800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C51\"\n                    data-col-index=\"2\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">7.3 10<sup>-6<\/sup> in\/in\/&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D51\"\n                    data-col-index=\"3\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25 - 400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E51\"\n                    data-col-index=\"4\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">13.5 10<sup>-6<\/sup> m\/m\/&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B52\"\n                    data-col-index=\"1\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75 - 1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C52\"\n                    data-col-index=\"2\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">7.7 10<sup>-6<\/sup> in\/in\/&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D52\"\n                    data-col-index=\"3\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25 - 500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E52\"\n                    data-col-index=\"4\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">13.9 10<sup>-6<\/sup> m\/m\/&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B53\"\n                    data-col-index=\"1\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75 - 1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C53\"\n                    data-col-index=\"2\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">8.2 10<sup>-6<\/sup> in\/in\/&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D53\"\n                    data-col-index=\"3\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25 - 600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E53\"\n                    data-col-index=\"4\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">14.3 10<sup>-6<\/sup> m\/m\/&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B54\"\n                    data-col-index=\"1\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75 - 1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C54\"\n                    data-col-index=\"2\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">8.5 10<sup>-6<\/sup> in\/in\/&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D54\"\n                    data-col-index=\"3\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25 - 700\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E54\"\n                    data-col-index=\"4\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">15.0 10<sup>-6<\/sup> m\/m\/&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B55\"\n                    data-col-index=\"1\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75 - 1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C55\"\n                    data-col-index=\"2\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">8.8 10<sup>-6<\/sup> in\/in\/&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D55\"\n                    data-col-index=\"3\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25 - 800\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E55\"\n                    data-col-index=\"4\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">15.5 10<sup>-6<\/sup> m\/m\/&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B56\"\n                    data-col-index=\"1\"\n                    data-row-index=\"55\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75 - 1800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C56\"\n                    data-col-index=\"2\"\n                    data-row-index=\"55\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">9.1 10<sup>-6<\/sup> in\/in\/&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D56\"\n                    data-col-index=\"3\"\n                    data-row-index=\"55\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25 - 900\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E56\"\n                    data-col-index=\"4\"\n                    data-row-index=\"55\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">16.0 10<sup>-6<\/sup> m\/m\/&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B57\"\n                    data-col-index=\"1\"\n                    data-row-index=\"56\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C57\"\n                    data-col-index=\"2\"\n                    data-row-index=\"56\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D57\"\n                    data-col-index=\"3\"\n                    data-row-index=\"56\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25 - 1000\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E57\"\n                    data-col-index=\"4\"\n                    data-row-index=\"56\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">16.5 10<sup>-6<\/sup> m\/m\/&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"11\"                     data-cell-id=\"A58\"\n                    data-col-index=\"0\"\n                    data-row-index=\"57\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Dynamic Modulus\nof Elasticity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B58\"\n                    data-col-index=\"1\"\n                    data-row-index=\"57\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C58\"\n                    data-col-index=\"2\"\n                    data-row-index=\"57\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">33.7 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D58\"\n                    data-col-index=\"3\"\n                    data-row-index=\"57\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E58\"\n                    data-col-index=\"4\"\n                    data-row-index=\"57\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        232 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B59\"\n                    data-col-index=\"1\"\n                    data-row-index=\"58\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C59\"\n                    data-col-index=\"2\"\n                    data-row-index=\"58\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">32.9 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D59\"\n                    data-col-index=\"3\"\n                    data-row-index=\"58\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E59\"\n                    data-col-index=\"4\"\n                    data-row-index=\"58\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        226 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B60\"\n                    data-col-index=\"1\"\n                    data-row-index=\"59\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C60\"\n                    data-col-index=\"2\"\n                    data-row-index=\"59\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">31.8 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D60\"\n                    data-col-index=\"3\"\n                    data-row-index=\"59\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E60\"\n                    data-col-index=\"4\"\n                    data-row-index=\"59\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        220 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B61\"\n                    data-col-index=\"1\"\n                    data-row-index=\"60\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C61\"\n                    data-col-index=\"2\"\n                    data-row-index=\"60\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">30.8 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D61\"\n                    data-col-index=\"3\"\n                    data-row-index=\"60\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E61\"\n                    data-col-index=\"4\"\n                    data-row-index=\"60\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        213 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B62\"\n                    data-col-index=\"1\"\n                    data-row-index=\"61\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C62\"\n                    data-col-index=\"2\"\n                    data-row-index=\"61\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">29.5 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D62\"\n                    data-col-index=\"3\"\n                    data-row-index=\"61\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E62\"\n                    data-col-index=\"4\"\n                    data-row-index=\"61\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        206 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B63\"\n                    data-col-index=\"1\"\n                    data-row-index=\"62\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C63\"\n                    data-col-index=\"2\"\n                    data-row-index=\"62\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">28.6 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D63\"\n                    data-col-index=\"3\"\n                    data-row-index=\"62\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E63\"\n                    data-col-index=\"4\"\n                    data-row-index=\"62\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        198 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B64\"\n                    data-col-index=\"1\"\n                    data-row-index=\"63\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C64\"\n                    data-col-index=\"2\"\n                    data-row-index=\"63\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">27.1 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D64\"\n                    data-col-index=\"3\"\n                    data-row-index=\"63\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E64\"\n                    data-col-index=\"4\"\n                    data-row-index=\"63\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        189 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B65\"\n                    data-col-index=\"1\"\n                    data-row-index=\"64\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C65\"\n                    data-col-index=\"2\"\n                    data-row-index=\"64\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">25.6 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D65\"\n                    data-col-index=\"3\"\n                    data-row-index=\"64\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        700\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E65\"\n                    data-col-index=\"4\"\n                    data-row-index=\"64\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        180 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B66\"\n                    data-col-index=\"1\"\n                    data-row-index=\"65\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C66\"\n                    data-col-index=\"2\"\n                    data-row-index=\"65\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">24.0 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D66\"\n                    data-col-index=\"3\"\n                    data-row-index=\"65\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E66\"\n                    data-col-index=\"4\"\n                    data-row-index=\"65\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        171 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B67\"\n                    data-col-index=\"1\"\n                    data-row-index=\"66\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C67\"\n                    data-col-index=\"2\"\n                    data-row-index=\"66\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">22.2 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D67\"\n                    data-col-index=\"3\"\n                    data-row-index=\"66\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E67\"\n                    data-col-index=\"4\"\n                    data-row-index=\"66\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        160 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B68\"\n                    data-col-index=\"1\"\n                    data-row-index=\"67\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C68\"\n                    data-col-index=\"2\"\n                    data-row-index=\"67\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">20.2 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D68\"\n                    data-col-index=\"3\"\n                    data-row-index=\"67\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E68\"\n                    data-col-index=\"4\"\n                    data-row-index=\"67\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        150 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"11\"                     data-cell-id=\"A69\"\n                    data-col-index=\"0\"\n                    data-row-index=\"68\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Dynamic Shear Modulus                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B69\"\n                    data-col-index=\"1\"\n                    data-row-index=\"68\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C69\"\n                    data-col-index=\"2\"\n                    data-row-index=\"68\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">13.0 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D69\"\n                    data-col-index=\"3\"\n                    data-row-index=\"68\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E69\"\n                    data-col-index=\"4\"\n                    data-row-index=\"68\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        90 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B70\"\n                    data-col-index=\"1\"\n                    data-row-index=\"69\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C70\"\n                    data-col-index=\"2\"\n                    data-row-index=\"69\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">12.5 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D70\"\n                    data-col-index=\"3\"\n                    data-row-index=\"69\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E70\"\n                    data-col-index=\"4\"\n                    data-row-index=\"69\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        88 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B71\"\n                    data-col-index=\"1\"\n                    data-row-index=\"70\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C71\"\n                    data-col-index=\"2\"\n                    data-row-index=\"70\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">12.0 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D71\"\n                    data-col-index=\"3\"\n                    data-row-index=\"70\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E71\"\n                    data-col-index=\"4\"\n                    data-row-index=\"70\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        86 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B72\"\n                    data-col-index=\"1\"\n                    data-row-index=\"71\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C72\"\n                    data-col-index=\"2\"\n                    data-row-index=\"71\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">11.4 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D72\"\n                    data-col-index=\"3\"\n                    data-row-index=\"71\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E72\"\n                    data-col-index=\"4\"\n                    data-row-index=\"71\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        83 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B73\"\n                    data-col-index=\"1\"\n                    data-row-index=\"72\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C73\"\n                    data-col-index=\"2\"\n                    data-row-index=\"72\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">10.9 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D73\"\n                    data-col-index=\"3\"\n                    data-row-index=\"72\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E73\"\n                    data-col-index=\"4\"\n                    data-row-index=\"72\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B74\"\n                    data-col-index=\"1\"\n                    data-row-index=\"73\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C74\"\n                    data-col-index=\"2\"\n                    data-row-index=\"73\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">10.3 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D74\"\n                    data-col-index=\"3\"\n                    data-row-index=\"73\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E74\"\n                    data-col-index=\"4\"\n                    data-row-index=\"73\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        76 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B75\"\n                    data-col-index=\"1\"\n                    data-row-index=\"74\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C75\"\n                    data-col-index=\"2\"\n                    data-row-index=\"74\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">9.7 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D75\"\n                    data-col-index=\"3\"\n                    data-row-index=\"74\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E75\"\n                    data-col-index=\"4\"\n                    data-row-index=\"74\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        73 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B76\"\n                    data-col-index=\"1\"\n                    data-row-index=\"75\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C76\"\n                    data-col-index=\"2\"\n                    data-row-index=\"75\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">9.0 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D76\"\n                    data-col-index=\"3\"\n                    data-row-index=\"75\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        700\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E76\"\n                    data-col-index=\"4\"\n                    data-row-index=\"75\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        69 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B77\"\n                    data-col-index=\"1\"\n                    data-row-index=\"76\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800\u00baF\u00a0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C77\"\n                    data-col-index=\"2\"\n                    data-row-index=\"76\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">8.3 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D77\"\n                    data-col-index=\"3\"\n                    data-row-index=\"76\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00baC\u00a0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E77\"\n                    data-col-index=\"4\"\n                    data-row-index=\"76\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65 GPa\u00a0                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B78\"\n                    data-col-index=\"1\"\n                    data-row-index=\"77\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C78\"\n                    data-col-index=\"2\"\n                    data-row-index=\"77\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">7.5 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D78\"\n                    data-col-index=\"3\"\n                    data-row-index=\"77\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E78\"\n                    data-col-index=\"4\"\n                    data-row-index=\"77\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B79\"\n                    data-col-index=\"1\"\n                    data-row-index=\"78\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00a0-                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C79\"\n                    data-col-index=\"2\"\n                    data-row-index=\"78\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00a0-                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D79\"\n                    data-col-index=\"3\"\n                    data-row-index=\"78\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00baC                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E79\"\n                    data-col-index=\"4\"\n                    data-row-index=\"78\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"11\"                     data-cell-id=\"A80\"\n                    data-col-index=\"0\"\n                    data-row-index=\"79\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Poisson's Ratio                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B80\"\n                    data-col-index=\"1\"\n                    data-row-index=\"79\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C80\"\n                    data-col-index=\"2\"\n                    data-row-index=\"79\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D80\"\n                    data-col-index=\"3\"\n                    data-row-index=\"79\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E80\"\n                    data-col-index=\"4\"\n                    data-row-index=\"79\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.30                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B81\"\n                    data-col-index=\"1\"\n                    data-row-index=\"80\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C81\"\n                    data-col-index=\"2\"\n                    data-row-index=\"80\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D81\"\n                    data-col-index=\"3\"\n                    data-row-index=\"80\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E81\"\n                    data-col-index=\"4\"\n                    data-row-index=\"80\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B82\"\n                    data-col-index=\"1\"\n                    data-row-index=\"81\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C82\"\n                    data-col-index=\"2\"\n                    data-row-index=\"81\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D82\"\n                    data-col-index=\"3\"\n                    data-row-index=\"81\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E82\"\n                    data-col-index=\"4\"\n                    data-row-index=\"81\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.27                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B83\"\n                    data-col-index=\"1\"\n                    data-row-index=\"82\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C83\"\n                    data-col-index=\"2\"\n                    data-row-index=\"82\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D83\"\n                    data-col-index=\"3\"\n                    data-row-index=\"82\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E83\"\n                    data-col-index=\"4\"\n                    data-row-index=\"82\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B84\"\n                    data-col-index=\"1\"\n                    data-row-index=\"83\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C84\"\n                    data-col-index=\"2\"\n                    data-row-index=\"83\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D84\"\n                    data-col-index=\"3\"\n                    data-row-index=\"83\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E84\"\n                    data-col-index=\"4\"\n                    data-row-index=\"83\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B85\"\n                    data-col-index=\"1\"\n                    data-row-index=\"84\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C85\"\n                    data-col-index=\"2\"\n                    data-row-index=\"84\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.31                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D85\"\n                    data-col-index=\"3\"\n                    data-row-index=\"84\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E85\"\n                    data-col-index=\"4\"\n                    data-row-index=\"84\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.30                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B86\"\n                    data-col-index=\"1\"\n                    data-row-index=\"85\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C86\"\n                    data-col-index=\"2\"\n                    data-row-index=\"85\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.32                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D86\"\n                    data-col-index=\"3\"\n                    data-row-index=\"85\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E86\"\n                    data-col-index=\"4\"\n                    data-row-index=\"85\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.31                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B87\"\n                    data-col-index=\"1\"\n                    data-row-index=\"86\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C87\"\n                    data-col-index=\"2\"\n                    data-row-index=\"86\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.32                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D87\"\n                    data-col-index=\"3\"\n                    data-row-index=\"86\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        700\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E87\"\n                    data-col-index=\"4\"\n                    data-row-index=\"86\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.32                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B88\"\n                    data-col-index=\"1\"\n                    data-row-index=\"87\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C88\"\n                    data-col-index=\"2\"\n                    data-row-index=\"87\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.33                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D88\"\n                    data-col-index=\"3\"\n                    data-row-index=\"87\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E88\"\n                    data-col-index=\"4\"\n                    data-row-index=\"87\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.32                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B89\"\n                    data-col-index=\"1\"\n                    data-row-index=\"88\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C89\"\n                    data-col-index=\"2\"\n                    data-row-index=\"88\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.33                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D89\"\n                    data-col-index=\"3\"\n                    data-row-index=\"88\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E89\"\n                    data-col-index=\"4\"\n                    data-row-index=\"88\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.33                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B90\"\n                    data-col-index=\"1\"\n                    data-row-index=\"89\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C90\"\n                    data-col-index=\"2\"\n                    data-row-index=\"89\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.34                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D90\"\n                    data-col-index=\"3\"\n                    data-row-index=\"89\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E90\"\n                    data-col-index=\"4\"\n                    data-row-index=\"89\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.33                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-80'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">RT = Room Temperature<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-low-cycle-fatigue-properties\">Low Cycle Fatigue Properties<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HAYNES<sup>\u00ae<\/sup> 188 alloy exhibits very good low cycle fatigue properties at elevated temperatures. Results shown below are for strain-controlled tests run in the temperature range from 800\u00b0F (425\u00b0C) to 1600\u00b0F (870\u00b0C). Samples were machined from bar. Tests were run with fully reversed strain (R = -1) at a frequency of 20 cpm (0.33 Hz).<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"680\" height=\"336\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-low-cycle-fatigue.jpg?resize=680%2C336&#038;ssl=1\" alt=\"\" class=\"wp-image-2164\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-low-cycle-fatigue.jpg?w=680&amp;ssl=1 680w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-low-cycle-fatigue.jpg?resize=300%2C148&amp;ssl=1 300w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-low-cycle-fatigue.jpg?resize=620%2C306&amp;ssl=1 620w\" sizes=\"(max-width: 680px) 100vw, 680px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-comparative-low-cycle-fatigue-properties\">Comparative Low Cycle Fatigue Properties.<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">The graph below compares the low cycle fatigue lives of a number of alloys tested at 800\u00b0F (425\u00b0C) in both the as-received and 1400\u00b0F (760\u00b0C)\/1000 hour pre-exposed condition. Samples were machined from plate or bar, after exposure for exposed samples. Tests were again run with fully reversed strain (R = -1) at a frequency of 20 cpm (0.33 Hz). TSR = Total Strain Range.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"682\" height=\"318\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparative-low-cycle-fatigue-properties.jpg?resize=682%2C318&#038;ssl=1\" alt=\"\" class=\"wp-image-2168\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparative-low-cycle-fatigue-properties.jpg?w=682&amp;ssl=1 682w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparative-low-cycle-fatigue-properties.jpg?resize=300%2C140&amp;ssl=1 300w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparative-low-cycle-fatigue-properties.jpg?resize=620%2C289&amp;ssl=1 620w\" sizes=\"(max-width: 682px) 100vw, 682px\" \/><\/figure>\n<\/div><\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-oxidation-resistance\">Oxidation Resistance<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HAYNES<sup>\u00ae<\/sup> 188 alloy exhibits very good resistance to both air and combustion gas oxidizing environments, and can be used for long-term continuous exposure at temperatures up to 2000\u00b0F (1095\u00b0C). For exposures of short duration, 188 alloy can be used at higher temperatures.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"752\" height=\"206\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-oxidation-figure.jpg?resize=752%2C206&#038;ssl=1\" alt=\"\" class=\"wp-image-2172\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-oxidation-figure.jpg?w=752&amp;ssl=1 752w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-oxidation-figure.jpg?resize=300%2C82&amp;ssl=1 300w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-oxidation-figure.jpg?resize=620%2C170&amp;ssl=1 620w\" sizes=\"(max-width: 752px) 100vw, 752px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-comparative-oxidation-resistance-in-flowing-air-1008-hours\">Comparative Oxidation Resistance in Flowing Air, 1008 Hours<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-59\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"13\"\n           data-rows=\"8\"\n           data-wpID=\"59\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        Alloy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:30.769230769231%;                    padding:10px;\n                    \"\n                    >\n                                        1800\u00b0F (980\u00b0C)                    <\/td>\n                                                                                    <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:30.769230769231%;                    padding:10px;\n                    \"\n                    >\n                                        2000\u00b0F (1095\u00b0C)                    <\/td>\n                                                                                    <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"J1\"\n                    data-col-index=\"9\"\n                    data-row-index=\"0\"\n                    style=\" width:30.769230769231%;                    padding:10px;\n                    \"\n                    >\n                                        2100\u00b0F (1150\u00b0C)                    <\/td>\n                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Average Metal Affected**                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Metal Loss                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Average Metal Affected**                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Metal Loss                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"J2\"\n                    data-col-index=\"9\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Average Metal Affected**                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"L2\"\n                    data-col-index=\"11\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Metal Loss                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"K3\"\n                    data-col-index=\"10\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"L3\"\n                    data-col-index=\"11\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"M3\"\n                    data-col-index=\"12\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        188                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.1                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.1                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.7                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        94                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.7                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"K4\"\n                    data-col-index=\"10\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        272                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"L4\"\n                    data-col-index=\"11\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.6                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"M4\"\n                    data-col-index=\"12\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        218                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        230<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        84                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K5\"\n                    data-col-index=\"10\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        112                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L5\"\n                    data-col-index=\"11\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M5\"\n                    data-col-index=\"12\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        X                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        112                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        33                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K6\"\n                    data-col-index=\"10\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        115                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L6\"\n                    data-col-index=\"11\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M6\"\n                    data-col-index=\"12\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        91                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        48                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        198                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        89                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K7\"\n                    data-col-index=\"10\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        513                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L7\"\n                    data-col-index=\"11\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M7\"\n                    data-col-index=\"12\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        465                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        617                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        51                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        97                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K8\"\n                    data-col-index=\"10\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        132                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L8\"\n                    data-col-index=\"11\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M8\"\n                    data-col-index=\"12\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-59'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEEF1 { background-color: #EEEEF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Flowing air at a velocity of 7.0 ft\/min (213.4 cm\/min) past the samples. Samples cycled to room temperature once per week.<br>**Metal Loss + Average Internal Penetration<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-oxidation-test-parameters\">Oxidation Test Parameters<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Burner rig oxidation tests were conducted by exposing sampIes 3\/8 in. x 2.5 in. x thickness (9 mm x 64 mm x thickness), in a rotating holder, to products of combustion of No. 2 fuel oil burned at a ratio of air to fuel of about 50:1. (Gas velocity was about 0.3 mach). Samples were automatically removed from the gas stream every 30 minutes and fan-cooled to near ambient temperature and then reinserted into the flame tunnel.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-comparative-burner-rig-oxidation-resistance-1000-hour-exposure-at-1800-f-980-c\">Comparative Burner Rig Oxidation Resistance 1000 Hour Exposure at 1800\u00b0F (980\u00b0C)<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-60\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"7\"\n           data-rows=\"8\"\n           data-wpID=\"60\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"7\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        1000 Hour Exposure at 1800\u00b0F (980\u00b0C), 30 Minute Cycles                    <\/td>\n                                                                                                                <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Alloy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Metal Loss                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Average Metal Affected                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Maximum Metal Affected                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        188                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.1                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.2                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        81                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.9                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        99                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        230<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        71                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        142                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        163                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        617                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        145                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        175                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        94                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        152                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        168                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        X                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        109                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        185                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        203                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-60'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEEF1 { background-color: #EEEEF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n.wpdt-bc-FFFFFF { background-color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-comparative-burner-rig-oxidation-resistance-at-2000\u00baf-1095\u00bac-for-500-hours\">Comparative Burner Rig Oxidation Resistance at 2000\u00baF (1095\u00baC) for 500 Hours<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-62\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"7\"\n           data-rows=\"8\"\n           data-wpID=\"62\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"7\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        500 Hour Exposure at 2000\u00b0F (1095\u00b0C), 30 Minute Cycles                    <\/td>\n                                                                                                                <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Alloy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Average Metal Loss Per Side                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Average Metal Affected                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Maximum Metal Affected                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        230<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        180                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        251                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        188                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.9                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        277                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.1                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        333                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14.1                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        358                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        X                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        295                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        356                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        384                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        617                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        338                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        531                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"6\"  rowspan=\"1\"                     data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Consumed                    <\/td>\n                                                                                                    <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-62'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEEF1 { background-color: #EEEEF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">&nbsp;<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"479\" height=\"286\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparative-burner-rig.png?resize=479%2C286&#038;ssl=1\" alt=\"\" class=\"wp-image-2176\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparative-burner-rig.png?w=479&amp;ssl=1 479w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparative-burner-rig.png?resize=300%2C179&amp;ssl=1 300w\" sizes=\"(max-width: 479px) 100vw, 479px\" \/><\/figure>\n<\/div>\n\n\n<p class=\"wp-block-paragraph\">*625 was consumed<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-water-vapor-oxidation-data\">Water Vapor Oxidation Data<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-66\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"5\"\n           data-rows=\"13\"\n           data-wpID=\"66\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"5\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">Air + 20% H<sub>2<\/sub>O at 1800&deg;F (982&deg;C), 1008 hours, cycled weekly<\/div>                    <\/td>\n                                                                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Alloy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Metal Loss                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Average Metal Affected                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        214<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.64                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        230<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.59                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.36                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.66                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        42                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        188                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.18                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00a05                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00a01.48                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        X                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.77                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        617                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.39                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.99                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        556<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.35                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.85                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HR\u2010120<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.38                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        53                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800HT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.47                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.07                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        129                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HR\u2010160<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.77                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.57                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        141                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-66'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEEF1 { background-color: #EEEEF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n.wpdt-bc-FFFFFF { background-color: #FFFFFF !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-hot-corrosion-resistance\">Hot Corrosion Resistance<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HAYNES<sup>\u00ae<\/sup> 188 alloy exhibits excellent resistance to sulfate deposit type hot corrosion. Tests were conducted in a low velocity burner rig burning No. 2 Fuel oil with 0.4 percent sulfur. The air:fuel ratio was 30:1. Artificial sea water was injected at a rate equivalent to 5 ppm salt. Tests were run for 1000 hours, with samples cycled out of the gas stream once an hour and cooled to near ambient temperature. Gas velocity was 13 ft.\/ sec. (4 m\/s).<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-hot-corrosion-resistance-at-1650-f-900-c\">Hot Corrosion Resistance at 1650\u00b0F (900\u00b0C)<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-56\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"5\"\n           data-rows=\"6\"\n           data-wpID=\"56\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Alloy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Metal Loss                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Average Metal Affected                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        188                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.8                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.7                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        69                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        230<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        130                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        132                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        X                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        41                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        140                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-56'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n.wpdt-bc-FFFFFF { background-color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-schematic-representation-of-metallographic-technique-used-for-evaluating-environmental-tests\">Schematic Representation of Metallographic Technique<br>Used for Evaluating Environmental Tests<\/h3>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"1085\" height=\"310\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation.png?resize=1085%2C310&#038;ssl=1\" alt=\"\" class=\"wp-image-2180\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation.png?w=1085&amp;ssl=1 1085w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation.png?resize=300%2C86&amp;ssl=1 300w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation.png?resize=1024%2C293&amp;ssl=1 1024w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation.png?resize=768%2C219&amp;ssl=1 768w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation.png?resize=620%2C177&amp;ssl=1 620w\" sizes=\"(max-width: 1085px) 100vw, 1085px\" \/><\/figure>\n<\/div><\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-sulfidation-resistance\">Sulfidation Resistance<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HAYNES<sup>\u00ae<\/sup> 188 alloy has very good resistance to gaseous sulfidation envronments encountered in various industrial applications. Tests were conducted at 1400\u00b0F (760\u00b0C) in a gas mixture consisting of 5 percent H<sub>2<\/sub>, 5 percent CO<sub>1<\/sub>, 1 percent CO<sub>2<\/sub> , and 0.15 percent H<sub>2<\/sub>S, balance Ar. Coupons were exposed for 215 hours. This is a severe test, with equilibrium sulfur partial pressure of 10<sup>-6<\/sup> to 10<sup>-7<\/sup> and oxygen partial pressures less than that needed to produce protective chromium oxide scales.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-sulfidation-resistance-at-1400-f-760-c\">Sulfidation Resistance at 1400\u00b0F (760\u00b0C)<\/h3>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"726\" height=\"288\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation-resistance.jpg?resize=726%2C288&#038;ssl=1\" alt=\"\" class=\"wp-image-2184\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation-resistance.jpg?w=726&amp;ssl=1 726w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation-resistance.jpg?resize=300%2C119&amp;ssl=1 300w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation-resistance.jpg?resize=620%2C246&amp;ssl=1 620w\" sizes=\"(max-width: 726px) 100vw, 726px\" \/><\/figure>\n<\/div>\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-71\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"9\"\n           data-rows=\"12\"\n           data-wpID=\"71\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"9\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">215 hours in an atmosphere of 5% H<sub>2<\/sub> + 5% CO + 0.15% H<sub>2<\/sub>S + Balance Ar<\/div>                    <\/td>\n                                                                                                                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Alloy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F (760\u00b0C)                    <\/td>\n                                                                                    <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F (871\u00b0C)                    <\/td>\n                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Metal Loss                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Average Metal Affected                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Metal Loss                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Average Metal Affected                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1 wpdt-tc-444444\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEEE wpdt-tc-444444\"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEEE wpdt-tc-444444\"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEEE wpdt-tc-444444\"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEEE wpdt-tc-444444\"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEEE wpdt-tc-444444\"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEEE wpdt-tc-444444\"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEEE wpdt-tc-444444\"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEEE wpdt-tc-444444\"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b5m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        135                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        188                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.6                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        41                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.3                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        84                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.7                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.7                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        145                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        556<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        124                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        157                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        417                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        310                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        157                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        231                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        211                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        358                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        617                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        127                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        274                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        97                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        437                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800H                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        180                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        284                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        201                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        >27.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        >701                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        168                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        320                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Partially Consumed                    <\/td>\n                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-FFFFFF\"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        X                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        >29.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        >749                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        >21.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        >551                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-71'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEEF1 { background-color: #EEEEF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n.wpdt-bc-EEEEEE { background-color: #EEEEEE !important;}\n.wpdt-bc-FFFFFF { background-color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-schematic-representation-of-metallographic-technique-used-for-evaluating-environmental-tests-0\">Schematic Representation of Metallographic Technique<br>Used for Evaluating Environmental Tests<\/h3>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"1085\" height=\"310\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation.png?resize=1085%2C310&#038;ssl=1\" alt=\"\" class=\"wp-image-2180\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation.png?w=1085&amp;ssl=1 1085w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation.png?resize=300%2C86&amp;ssl=1 300w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation.png?resize=1024%2C293&amp;ssl=1 1024w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation.png?resize=768%2C219&amp;ssl=1 768w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-sulfidation.png?resize=620%2C177&amp;ssl=1 620w\" sizes=\"(max-width: 1085px) 100vw, 1085px\" \/><\/figure>\n<\/div><\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-fabrication-characteristics\">Fabrication Characteristics<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HAYNES<sup>\u00ae<\/sup> 188 alloy is normally solution heat treated in the range of 2125-2175\u00b0F for a time to commensurate with section thickness. Annealing during fabrication can be performed at even lower temperatures, but a final, subsequent solution heat treatment is needed to produce optimum properties and structure.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-effect-of-cold-reduction-upon-room-temperature-properties\">Effect of Cold Reduction Upon Room-Temperature Properties*<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-53\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"8\"\n           data-rows=\"19\"\n           data-wpID=\"53\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        Cold\nReduction                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        Subsequent Temperature                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        0.2%\nYield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate\nTensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        Hardness                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HR BW\/C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"5\"                     data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        None                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        460                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        137.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        945                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        98.1 HRBW                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        105.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        730                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        151.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1045                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        32.1 HRC                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        132.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        915                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        165.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1145                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        37.1 HRC                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        167.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1150                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        195.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1345                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        41.2 HRC                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        176.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1220                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        214.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1480                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43.5 HRC                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1950\u00b0F (1065\u00b0C)\nfor 5 min.                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        91.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        630                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        148.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1025                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        41.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        29.7 HRC                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        87.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        605                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        153.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1055                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        41.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        27.8 HRC                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        84.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        580                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        158.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1090                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        41.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        29.6 HRC                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        90.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        162.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1120                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        39.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        31.1 HRC                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2050\u00b0F (1120\u00b0C)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        64.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        445                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        143.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        985                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21.9 HRC                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        71.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        490                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        149.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1025                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24.5 HRC                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A14\"\n                    data-col-index=\"0\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        555                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        155.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1070                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        27.6 HRC                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A15\"\n                    data-col-index=\"0\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        86.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        159.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1095                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        29.5 HRC                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2150\u00b0F (1175\u00b0C)\nfor 5 min.                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        425                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        139.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        965                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        95.6 HRBW                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A17\"\n                    data-col-index=\"0\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        64.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        445                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        141.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        975                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        53.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H17\"\n                    data-col-index=\"7\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        97.1 HRBW                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A18\"\n                    data-col-index=\"0\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        460                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        142.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F18\"\n                    data-col-index=\"5\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        985                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G18\"\n                    data-col-index=\"6\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        51.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H18\"\n                    data-col-index=\"7\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        98.5 HRBW                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A19\"\n                    data-col-index=\"0\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C19\"\n                    data-col-index=\"2\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        64.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        440                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        141.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F19\"\n                    data-col-index=\"5\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        975                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G19\"\n                    data-col-index=\"6\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H19\"\n                    data-col-index=\"7\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        97.2 HRBW                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-53'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEEF1 { background-color: #EEEEF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Based upon rolling reduction taken upon 0.125 in. (3.2 mm) thick sheet. Duplicate tests.<br>HRC = Hardness Rockwell \u201cC\u201d.<br>HRBW= Hardness Rockwell &#8220;B&#8221;, Tungsten Indentor.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-welding\">Welding<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HAYNES<sup>\u00ae<\/sup> 188 alloy is readily welded by Gas Tungsten Arc (GTAW), Gas Metal Arc (GMAW), Shielded Metal Arc (SMAW), electron bean welding, and resistance welding techniques. Its welding characteristics are similar to those of HAYNES<sup>\u00ae<\/sup> 25 alloy. Submerged Arc welding is not recommended, as this process is characterized by high heat input to the base metal and slow cooling of the weld. These factors can increase weld restraint and promote cracking.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-base-metal-preparation\">Base Metal Preparation<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">The joint surface and adjacent area should be thoroughly cleaned before welding. All grease, oil, crayon marks, sulfur compounds, and other foreign matter should be removed. Contact with copper or copper-bearing materials in the joint area should be avoided. It is preferable, but not necessary, that the alloy be in the solution-annealed condition when welded.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-filler-metal-selection\">Filler Metal Selection<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Matching composition filler metal is recommended for joining alloy 188. For joining section thicknesses greater than 3\/8 inch (9.5 mm), HAYNES<sup>\u00ae<\/sup> 230-W<sup>\u00ae<\/sup> filler wire (AWS A5.14 ERNiCrWMo-1) is suggested. For shielded metal arc welding, HAYNES<sup>\u00ae<\/sup> 25 alloy electrodes (AMS 5797) are suggested. For dissimilar joining of 188 alloy to nickel-, cobalt-, or iron- base materials, 188 alloy itself, 230-W<sup>\u00ae<\/sup> filler wire, HAYNES<sup>\u00ae<\/sup> 556<sup>\u00ae<\/sup> alloy (AMS 5831), HASTELLOY<sup>\u00ae<\/sup> S alloy (AMS 5838), or HASTELLOY<sup>\u00ae<\/sup> W alloy (AMS 5786) welding products are suggested, depending upon the particular case. Please <a href=\"\/datasheet\/welding-and-joining\" target=\"_blank\" rel=\"noopener\">click here<\/a> or see the <a href=\"https:\/\/wsg.haynesintl.com\/SmartGuide\/MainMenu.aspx\" target=\"_blank\" rel=\"noreferrer noopener\">Haynes Welding SmartGuide<\/a> for more information.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-preheating-interpass-temperatures-and-postweld-heat-treatment\">Preheating, Interpass Temperatures, and Postweld Heat Treatment<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Preheat is not required. Preheat is generally specified as room temperature (typical shop conditions). Interpass temperature should be maintained below 200\u00b0F (93\u00b0C). Auxiliary cooling methods may be used between weld passes, as needed, providing that such methods do not introduce contaminants. Postweld heat treatment is not generally required for 188 alloy. For further information, please <a href=\"\/datasheet\/welding-and-fabrication\" target=\"_blank\" rel=\"noopener\">click here<\/a>.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-welded-tensile-room-temperature\">Welded Tensile \u2013 Room Temperature<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-87\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"6\"\n           data-rows=\"5\"\n           data-wpID=\"87\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:16.666666666667%;                    padding:10px;\n                    \"\n                    >\n                                        Condition                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:33.333333333333%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:33.333333333333%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate Tensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:16.666666666667%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        68                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        469                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        133                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        917                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Welded Transverse                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        483                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        123                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        848                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        31                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        All Weld Metal                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        545                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        117                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        807                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-87'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEEF1 { background-color: #EEEEF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-machining\">Machining<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Machining information can be found <a href=\"https:\/\/haynesintl.com\/zh-hans\/alloys\/%e7%84%8a%e6%8e%a5%e4%b8%8e%e5%88%b6%e9%80%a0\/\">here<\/a>.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-specifications-and-codes\">Specifications and Codes<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-68\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"2\"\n           data-rows=\"11\"\n           data-wpID=\"68\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        HAYNES<sup>\u00ae<\/sup> 188 alloy (R30188)                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet, Plate & Strip                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        AMS 5608                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Billet, Rod & Bar                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        AMS 5772                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Coated Electrodes                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Bare Welding Rods & Wire                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Seamless Pipe & Tube                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Welded Pipe & Tube                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Fittings                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Forgings                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        AMS 5772                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        DIN                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Others                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-68'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-codes\">Codes<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-70\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"2\"\n           data-rows=\"2\"\n           data-wpID=\"70\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        HAYNES<sup>\u00ae<\/sup> 188 alloy (R30188)                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MMPDS                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.4.2                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-70'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-disclaimer\">Disclaimer<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Haynes International makes all reasonable efforts to ensure the accuracy and correctness of the data displayed on this site but makes no representations or warranties as to the data\u2019s accuracy, correctness or reliability. All data are for general information only and not for providing design advice. Alloy properties disclosed here are based on work conducted principally by Haynes International, Inc. and occasionally supplemented by information from the open literature and, as such, are indicative only of the results of such tests and should not be considered guaranteed maximums or minimums.  It is the responsibility of the user to test specific alloys under actual service conditions to determine their suitability for a particular purpose.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">For specific concentrations of elements present in a particular product and a discussion of the potential health affects thereof, refer to the Safety Data Sheets supplied by Haynes International, Inc.  All trademarks are owned by Haynes International, Inc., unless otherwise indicated.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-alloy-brochure\">Alloy Brochure<\/h2>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-brochure.pdf\">Download<\/a><\/div>\n<\/div>\n<\/div><\/div>\n","protected":false},"excerpt":{"rendered":"<p>Principal Features HAYNES<sup>\u00ae<\/sup> 188 alloy (UNS R30188) is a  [\u2026]<\/p>\n","protected":false},"author":2,"featured_media":0,"parent":13036,"menu_order":2,"template":"","meta":{"_acf_changed":false,"_searchwp_excluded":"","inline_featured_image":false,"footnotes":""},"class_list":["post-13067","alloys","type-alloys","status-publish","hentry"],"acf":[],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v27.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>HAYNES\u00ae 188 \u5408\u91d1 - Haynes International<\/title>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/haynesintl.com\/zh-hans\/alloys\/\u5408\u91d1\u76ee\u5f55\/\u9ad8\u6e29\u5408\u91d1\/haynes-188-\u5408\u91d1\/\" \/>\n<meta property=\"og:locale\" content=\"zh_CN\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"HAYNES\u00ae 188 \u5408\u91d1\" \/>\n<meta property=\"og:description\" content=\"Principal Features HAYNES\u00ae 188 alloy (UNS R30188) is a [\u2026]\" \/>\n<meta property=\"og:url\" content=\"https:\/\/haynesintl.com\/zh-hans\/alloys\/\u5408\u91d1\u76ee\u5f55\/\u9ad8\u6e29\u5408\u91d1\/haynes-188-\u5408\u91d1\/\" \/>\n<meta property=\"og:site_name\" content=\"Haynes International\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/HaynesInternationalInc\/\" \/>\n<meta property=\"article:modified_time\" content=\"2025-02-24T13:51:36+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparison-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours.png\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:site\" content=\"@HaynesIntl\" \/>\n<meta name=\"twitter:label1\" content=\"\u9884\u8ba1\u9605\u8bfb\u65f6\u95f4\" \/>\n\t<meta name=\"twitter:data1\" content=\"10 \u5206\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/zh-hans\\\/alloys\\\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\\\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\\\/haynes-188-%e5%90%88%e9%87%91\\\/\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/zh-hans\\\/alloys\\\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\\\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\\\/haynes-188-%e5%90%88%e9%87%91\\\/\",\"name\":\"HAYNES\u00ae 188 \u5408\u91d1 - Haynes International\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/zh-hans\\\/alloys\\\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\\\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\\\/haynes-188-%e5%90%88%e9%87%91\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/zh-hans\\\/alloys\\\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\\\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\\\/haynes-188-%e5%90%88%e9%87%91\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/188-comparison-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours.png\",\"datePublished\":\"2024-08-06T16:16:31+00:00\",\"dateModified\":\"2025-02-24T13:51:36+00:00\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/zh-hans\\\/alloys\\\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\\\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\\\/haynes-188-%e5%90%88%e9%87%91\\\/#breadcrumb\"},\"inLanguage\":\"zh-Hans\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/haynesintl.com\\\/zh-hans\\\/alloys\\\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\\\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\\\/haynes-188-%e5%90%88%e9%87%91\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"zh-Hans\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/zh-hans\\\/alloys\\\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\\\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\\\/haynes-188-%e5%90%88%e9%87%91\\\/#primaryimage\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/188-comparison-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours.png\",\"contentUrl\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/188-comparison-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours.png\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/zh-hans\\\/alloys\\\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\\\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\\\/haynes-188-%e5%90%88%e9%87%91\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/zh-hans\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"\u5408\u91d1\u76ee\u5f55\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/zh-hans\\\/alloys\\\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\\\/\"},{\"@type\":\"ListItem\",\"position\":3,\"name\":\"\u9ad8\u6e29\u5408\u91d1\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/zh-hans\\\/alloys\\\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\\\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\\\/\"},{\"@type\":\"ListItem\",\"position\":4,\"name\":\"HAYNES\u00ae 188 \u5408\u91d1\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#website\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\",\"name\":\"Haynes International\",\"description\":\"The Home of HASTELLOY\u00ae and HAYNES\u00ae high-performance alloys\",\"publisher\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"zh-Hans\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#organization\",\"name\":\"Haynes International\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"zh-Hans\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/07\\\/logo.webp?fit=484%2C188&ssl=1\",\"contentUrl\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/07\\\/logo.webp?fit=484%2C188&ssl=1\",\"width\":484,\"height\":188,\"caption\":\"Haynes International\"},\"image\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/HaynesInternationalInc\\\/\",\"https:\\\/\\\/x.com\\\/HaynesIntl\",\"https:\\\/\\\/www.instagram.com\\\/haynesinternational\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/company\\\/haynes-international\\\/\"]}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"HAYNES\u00ae 188 \u5408\u91d1 - Haynes International","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/haynesintl.com\/zh-hans\/alloys\/\u5408\u91d1\u76ee\u5f55\/\u9ad8\u6e29\u5408\u91d1\/haynes-188-\u5408\u91d1\/","og_locale":"zh_CN","og_type":"article","og_title":"HAYNES\u00ae 188 \u5408\u91d1","og_description":"Principal Features HAYNES\u00ae 188 alloy (UNS R30188) is a [\u2026]","og_url":"https:\/\/haynesintl.com\/zh-hans\/alloys\/\u5408\u91d1\u76ee\u5f55\/\u9ad8\u6e29\u5408\u91d1\/haynes-188-\u5408\u91d1\/","og_site_name":"Haynes International","article_publisher":"https:\/\/www.facebook.com\/HaynesInternationalInc\/","article_modified_time":"2025-02-24T13:51:36+00:00","og_image":[{"url":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparison-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours.png","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_site":"@HaynesIntl","twitter_misc":{"\u9884\u8ba1\u9605\u8bfb\u65f6\u95f4":"10 \u5206"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"WebPage","@id":"https:\/\/haynesintl.com\/zh-hans\/alloys\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\/haynes-188-%e5%90%88%e9%87%91\/","url":"https:\/\/haynesintl.com\/zh-hans\/alloys\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\/haynes-188-%e5%90%88%e9%87%91\/","name":"HAYNES\u00ae 188 \u5408\u91d1 - Haynes International","isPartOf":{"@id":"https:\/\/haynesintl.com\/en\/#website"},"primaryImageOfPage":{"@id":"https:\/\/haynesintl.com\/zh-hans\/alloys\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\/haynes-188-%e5%90%88%e9%87%91\/#primaryimage"},"image":{"@id":"https:\/\/haynesintl.com\/zh-hans\/alloys\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\/haynes-188-%e5%90%88%e9%87%91\/#primaryimage"},"thumbnailUrl":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparison-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours.png","datePublished":"2024-08-06T16:16:31+00:00","dateModified":"2025-02-24T13:51:36+00:00","breadcrumb":{"@id":"https:\/\/haynesintl.com\/zh-hans\/alloys\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\/haynes-188-%e5%90%88%e9%87%91\/#breadcrumb"},"inLanguage":"zh-Hans","potentialAction":[{"@type":"ReadAction","target":["https:\/\/haynesintl.com\/zh-hans\/alloys\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\/haynes-188-%e5%90%88%e9%87%91\/"]}]},{"@type":"ImageObject","inLanguage":"zh-Hans","@id":"https:\/\/haynesintl.com\/zh-hans\/alloys\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\/haynes-188-%e5%90%88%e9%87%91\/#primaryimage","url":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparison-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours.png","contentUrl":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/188-comparison-of-sheet-materials-stress-to-produce-1-creep-in-1000-hours.png"},{"@type":"BreadcrumbList","@id":"https:\/\/haynesintl.com\/zh-hans\/alloys\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\/haynes-188-%e5%90%88%e9%87%91\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/haynesintl.com\/zh-hans\/"},{"@type":"ListItem","position":2,"name":"\u5408\u91d1\u76ee\u5f55","item":"https:\/\/haynesintl.com\/zh-hans\/alloys\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\/"},{"@type":"ListItem","position":3,"name":"\u9ad8\u6e29\u5408\u91d1","item":"https:\/\/haynesintl.com\/zh-hans\/alloys\/%e5%90%88%e9%87%91%e7%9b%ae%e5%bd%95\/%e9%ab%98%e6%b8%a9%e5%90%88%e9%87%91\/"},{"@type":"ListItem","position":4,"name":"HAYNES\u00ae 188 \u5408\u91d1"}]},{"@type":"WebSite","@id":"https:\/\/haynesintl.com\/en\/#website","url":"https:\/\/haynesintl.com\/en\/","name":"Haynes International","description":"The Home of HASTELLOY\u00ae and HAYNES\u00ae high-performance alloys","publisher":{"@id":"https:\/\/haynesintl.com\/en\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/haynesintl.com\/en\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"zh-Hans"},{"@type":"Organization","@id":"https:\/\/haynesintl.com\/en\/#organization","name":"Haynes International","url":"https:\/\/haynesintl.com\/en\/","logo":{"@type":"ImageObject","inLanguage":"zh-Hans","@id":"https:\/\/haynesintl.com\/en\/#\/schema\/logo\/image\/","url":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/07\/logo.webp?fit=484%2C188&ssl=1","contentUrl":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/07\/logo.webp?fit=484%2C188&ssl=1","width":484,"height":188,"caption":"Haynes International"},"image":{"@id":"https:\/\/haynesintl.com\/en\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/HaynesInternationalInc\/","https:\/\/x.com\/HaynesIntl","https:\/\/www.instagram.com\/haynesinternational\/","https:\/\/www.linkedin.com\/company\/haynes-international\/"]}]}},"jetpack_sharing_enabled":true,"_links":{"self":[{"href":"https:\/\/haynesintl.com\/zh-hans\/wp-json\/wp\/v2\/alloys\/13067","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/haynesintl.com\/zh-hans\/wp-json\/wp\/v2\/alloys"}],"about":[{"href":"https:\/\/haynesintl.com\/zh-hans\/wp-json\/wp\/v2\/types\/alloys"}],"author":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/zh-hans\/wp-json\/wp\/v2\/users\/2"}],"version-history":[{"count":1,"href":"https:\/\/haynesintl.com\/zh-hans\/wp-json\/wp\/v2\/alloys\/13067\/revisions"}],"predecessor-version":[{"id":13068,"href":"https:\/\/haynesintl.com\/zh-hans\/wp-json\/wp\/v2\/alloys\/13067\/revisions\/13068"}],"up":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/zh-hans\/wp-json\/wp\/v2\/alloys\/13036"}],"wp:attachment":[{"href":"https:\/\/haynesintl.com\/zh-hans\/wp-json\/wp\/v2\/media?parent=13067"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}