{"id":13496,"date":"2024-08-06T16:16:31","date_gmt":"2024-08-06T16:16:31","guid":{"rendered":"https:\/\/haynesintl.com\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/"},"modified":"2025-02-25T15:38:42","modified_gmt":"2025-02-25T15:38:42","slug":"hastelloy-x","status":"publish","type":"alloys","link":"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/","title":{"rendered":"HASTELLOY<sup>\u00ae<\/sup> X"},"content":{"rendered":"\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-principal-features\">Principal Features<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;X alloy (UNS N06002 (W86002) is a nickel-chromium-iron-molybdenum alloy that possesses an exceptional combination of oxidation resistance, fabricability and high-temperature strength. It has also been found to be exceptionally resistant to stress-corrosion cracking in petrochemical applications. X alloy exhibits good ductility after prolonged exposure at temperatures of 1200, 1400, 1600\u00b0F (650, 760 and 870\u00b0C) for 16,000 hours.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-ease-of-fabrication\">Ease of Fabrication<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup>\u00ae<\/sup> X alloy has excellent forming and welding characteristics. It may be forged or otherwise hot-worked, providing it is held at 2150\u00b0F (1177\u00b0C) for a time sufficient to bring the entire piece to temperature. As a consequence of its good ductility, HASTELLOY<sup>\u00ae<\/sup> X alloy is also readily formed by cold- working. All hot- or cold- worked parts should be annealed and rapidly cooled in order to restore the best balance of properties.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The alloy can be welded by a variety of techniques, including gas tungsten arc (GTAW), gas metal arc (GMAW), shielded metal arc (SMAW), and resistance welding.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Additional information regarding fabrication can be found&nbsp;<a href=\"https:\/\/haynesintl.com\/es\/alloys\/soldadura-y-fabricacion\/\" target=\"_blank\" rel=\"noopener\">here<\/a>.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-heat-treatment\">Heat Treatment<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Wrought forms of HASTELLOY<sup>\u00ae<\/sup>&nbsp;X alloy are furnished in the solution heat-treated condition unless otherwise specified. X alloy is typically solution heat-treated at 2150\u00b0F (1177\u00b0C) and rapid cooled. Bright annealed products are cooled in hydrogen.&nbsp; Annealing at temperatures lower than the solution heat- treating may cause precipitation of secondary phases, which may affect the alloy\u2019s strength and ductility.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-useful-for-aircraft-furnace-and-chemical-process-components\">Useful for Aircraft, Furnace and Chemical Process Components<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">X alloy has wide use in gas turbine engines for combustion zone components such as transition ducts, combustor cans, spray bars and flame holders as well as in afterburners, tailpipes and cabin heaters. It is recommended for use in industrial furnace applications because it has unusual resistant to oxidizing, reducing and neutral atmospheres. Furnace rolls of this alloy were still in good condition after operating for 8,700 hours at 2150\u00b0F (1177\u00b0C). HASTELLOY<sup>\u00ae<\/sup>&nbsp;X alloy is also used in the chemical process industry for retorts, muffles, catalyst support grids, furnace baffles, tubing for pyrolysis operations and flash drier components.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">*Please contact our\u00a0<a href=\"https:\/\/haynesintl.com\/es\/contacto\/apoyo-tecnico\/\" target=\"_blank\" rel=\"noopener\">technical support team<\/a>\u00a0if you have technical questions about this alloy.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-nominal-composition\">Nominal Composition<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-136\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"2\"\n           data-rows=\"14\"\n           data-wpID=\"136\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-tc-FFFFFF wpdt-bold wpdt-bc-063D71 wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:102.28310502283%;                    padding:10px;\n                    \"\n                    >\n                                        Weight %                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Nickel                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47 Balance                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Chromium                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22.0                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Iron                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18.0                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Molybdenum                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.0                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Cobalt                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Tungsten                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.6                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Carbon                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.1                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Manganese                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Silicon                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.0 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Boron                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.008 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Niobium                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5 max.\u00a0                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Aluminum                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5 max.\u00a0                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A14\"\n                    data-col-index=\"0\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Titanium                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15 max.\u00a0                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-136'>\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-bc-EEEEF1 { background-color: #EEEEF1 !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-creep-and-stress-rupture-strengths\">Creep and Stress-Rupture Strengths<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-minimum-creep-rate-hastelloy-nbsp-x-sheet-solution-annealed\">Minimum Creep Rate, HASTELLOY<sup>\u00ae<\/sup>&nbsp;X Sheet, Solution-Annealed<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-545\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"10\"\n           data-rows=\"8\"\n           data-wpID=\"545\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"8\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:80%;                    padding:10px;\n                    \"\n                    >\n                                        Average Stress for Indicated Percent\/Hour Minimum Creep Rate                    <\/td>\n                                                                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.0001                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.001                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.1                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        101                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        145                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        31.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        214                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        303                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        69                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        97                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        134                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        982                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1093                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-545'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-hastelloy-nbsp-x-plate-solution-annealed\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;X Plate, Solution-annealed<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-546\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"11\"\n           data-rows=\"30\"\n           data-wpID=\"546\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:18.181818181818%;                    padding:10px;\n                    \"\n                    >\n                                        Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:9.0909090909091%;                    padding:10px;\n                    \"\n                    >\n                                        Creep                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"8\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:72.727272727273%;                    padding:10px;\n                    \"\n                    >\n                                        Approximate Initial Stress to Produce Specified Creep in                    <\/td>\n                                                                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10 h                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100 h                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1,000 h                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"J2\"\n                    data-col-index=\"9\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10,000 h                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"K3\"\n                    data-col-index=\"10\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        27.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        188                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        128                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K4\"\n                    data-col-index=\"10\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        88                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        207                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        145                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K5\"\n                    data-col-index=\"10\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        448*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        345                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        36                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        248                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K6\"\n                    data-col-index=\"10\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        179                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1300                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        704                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        172                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        112                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K7\"\n                    data-col-index=\"10\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        57                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        186                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        131                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        97                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K8\"\n                    data-col-index=\"10\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        72                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        317                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        32                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        221                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        23                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        159                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K9\"\n                    data-col-index=\"10\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        117                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        103                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        71                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K10\"\n                    data-col-index=\"10\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        39                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        124                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        90                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K11\"\n                    data-col-index=\"10\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        207                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        146                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J12\"\n                    data-col-index=\"9\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K12\"\n                    data-col-index=\"10\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1500                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        816                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        68                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I13\"\n                    data-col-index=\"8\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        37                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J13\"\n                    data-col-index=\"9\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.85                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K13\"\n                    data-col-index=\"10\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        27                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        86                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I14\"\n                    data-col-index=\"8\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J14\"\n                    data-col-index=\"9\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K14\"\n                    data-col-index=\"10\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        32                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        141                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        103                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I15\"\n                    data-col-index=\"8\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        72                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J15\"\n                    data-col-index=\"9\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K15\"\n                    data-col-index=\"10\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        48                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        35                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I16\"\n                    data-col-index=\"8\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J16\"\n                    data-col-index=\"9\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K16\"\n                    data-col-index=\"10\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H17\"\n                    data-col-index=\"7\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I17\"\n                    data-col-index=\"8\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        31                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J17\"\n                    data-col-index=\"9\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K17\"\n                    data-col-index=\"10\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F18\"\n                    data-col-index=\"5\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G18\"\n                    data-col-index=\"6\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        69                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H18\"\n                    data-col-index=\"7\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I18\"\n                    data-col-index=\"8\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J18\"\n                    data-col-index=\"9\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K18\"\n                    data-col-index=\"10\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        31                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A19\"\n                    data-col-index=\"0\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1700                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B19\"\n                    data-col-index=\"1\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        927                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C19\"\n                    data-col-index=\"2\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        35                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F19\"\n                    data-col-index=\"5\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G19\"\n                    data-col-index=\"6\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H19\"\n                    data-col-index=\"7\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I19\"\n                    data-col-index=\"8\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J19\"\n                    data-col-index=\"9\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K19\"\n                    data-col-index=\"10\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.0                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F20\"\n                    data-col-index=\"5\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G20\"\n                    data-col-index=\"6\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H20\"\n                    data-col-index=\"7\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I20\"\n                    data-col-index=\"8\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J20\"\n                    data-col-index=\"9\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K20\"\n                    data-col-index=\"10\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C21\"\n                    data-col-index=\"2\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D21\"\n                    data-col-index=\"3\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E21\"\n                    data-col-index=\"4\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        69                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F21\"\n                    data-col-index=\"5\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G21\"\n                    data-col-index=\"6\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H21\"\n                    data-col-index=\"7\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I21\"\n                    data-col-index=\"8\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J21\"\n                    data-col-index=\"9\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K21\"\n                    data-col-index=\"10\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A22\"\n                    data-col-index=\"0\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B22\"\n                    data-col-index=\"1\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        982                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C22\"\n                    data-col-index=\"2\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D22\"\n                    data-col-index=\"3\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E22\"\n                    data-col-index=\"4\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F22\"\n                    data-col-index=\"5\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G22\"\n                    data-col-index=\"6\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H22\"\n                    data-col-index=\"7\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I22\"\n                    data-col-index=\"8\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J22\"\n                    data-col-index=\"9\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.55                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K22\"\n                    data-col-index=\"10\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.8                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C23\"\n                    data-col-index=\"2\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D23\"\n                    data-col-index=\"3\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E23\"\n                    data-col-index=\"4\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F23\"\n                    data-col-index=\"5\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G23\"\n                    data-col-index=\"6\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H23\"\n                    data-col-index=\"7\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.45                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I23\"\n                    data-col-index=\"8\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J23\"\n                    data-col-index=\"9\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.65                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K23\"\n                    data-col-index=\"10\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C24\"\n                    data-col-index=\"2\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D24\"\n                    data-col-index=\"3\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E24\"\n                    data-col-index=\"4\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F24\"\n                    data-col-index=\"5\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G24\"\n                    data-col-index=\"6\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H24\"\n                    data-col-index=\"7\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I24\"\n                    data-col-index=\"8\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J24\"\n                    data-col-index=\"9\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K24\"\n                    data-col-index=\"10\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A25\"\n                    data-col-index=\"0\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1900                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B25\"\n                    data-col-index=\"1\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1038                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C25\"\n                    data-col-index=\"2\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D25\"\n                    data-col-index=\"3\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E25\"\n                    data-col-index=\"4\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F25\"\n                    data-col-index=\"5\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G25\"\n                    data-col-index=\"6\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H25\"\n                    data-col-index=\"7\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.55                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I25\"\n                    data-col-index=\"8\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J25\"\n                    data-col-index=\"9\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K25\"\n                    data-col-index=\"10\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C26\"\n                    data-col-index=\"2\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D26\"\n                    data-col-index=\"3\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E26\"\n                    data-col-index=\"4\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F26\"\n                    data-col-index=\"5\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G26\"\n                    data-col-index=\"6\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H26\"\n                    data-col-index=\"7\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.65                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I26\"\n                    data-col-index=\"8\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J26\"\n                    data-col-index=\"9\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K26\"\n                    data-col-index=\"10\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C27\"\n                    data-col-index=\"2\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D27\"\n                    data-col-index=\"3\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E27\"\n                    data-col-index=\"4\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F27\"\n                    data-col-index=\"5\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G27\"\n                    data-col-index=\"6\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H27\"\n                    data-col-index=\"7\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I27\"\n                    data-col-index=\"8\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J27\"\n                    data-col-index=\"9\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K27\"\n                    data-col-index=\"10\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A28\"\n                    data-col-index=\"0\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B28\"\n                    data-col-index=\"1\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1093                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C28\"\n                    data-col-index=\"2\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D28\"\n                    data-col-index=\"3\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E28\"\n                    data-col-index=\"4\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F28\"\n                    data-col-index=\"5\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G28\"\n                    data-col-index=\"6\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H28\"\n                    data-col-index=\"7\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I28\"\n                    data-col-index=\"8\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.0*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J28\"\n                    data-col-index=\"9\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K28\"\n                    data-col-index=\"10\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C29\"\n                    data-col-index=\"2\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D29\"\n                    data-col-index=\"3\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E29\"\n                    data-col-index=\"4\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F29\"\n                    data-col-index=\"5\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G29\"\n                    data-col-index=\"6\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H29\"\n                    data-col-index=\"7\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.20*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I29\"\n                    data-col-index=\"8\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.4*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J29\"\n                    data-col-index=\"9\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K29\"\n                    data-col-index=\"10\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C30\"\n                    data-col-index=\"2\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D30\"\n                    data-col-index=\"3\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E30\"\n                    data-col-index=\"4\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F30\"\n                    data-col-index=\"5\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G30\"\n                    data-col-index=\"6\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H30\"\n                    data-col-index=\"7\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.60*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I30\"\n                    data-col-index=\"8\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.1*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J30\"\n                    data-col-index=\"9\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K30\"\n                    data-col-index=\"10\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-546'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Significant extrapolation<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-hastelloy-nbsp-x-sheet-solution-annealed\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;X Sheet, Solution-annealed<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-547\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"11\"\n           data-rows=\"30\"\n           data-wpID=\"547\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:18.181818181818%;                    padding:10px;\n                    \"\n                    >\n                                        Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:9.0909090909091%;                    padding:10px;\n                    \"\n                    >\n                                        Creep                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"8\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:72.727272727273%;                    padding:10px;\n                    \"\n                    >\n                                        Approximate Initial Stress to Produce Specified Creep in                    <\/td>\n                                                                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10 h                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100 h                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1,000 h                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"J2\"\n                    data-col-index=\"9\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10,000 h                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"K3\"\n                    data-col-index=\"10\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        178                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        124                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K4\"\n                    data-col-index=\"10\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        193                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        145                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K5\"\n                    data-col-index=\"10\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        455*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        48                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        331                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        35                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        241                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K6\"\n                    data-col-index=\"10\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        179                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1300                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        704                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        23.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        162                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        112                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        83                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K7\"\n                    data-col-index=\"10\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        179                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        131                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        97                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K8\"\n                    data-col-index=\"10\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        303                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        32                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        221                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        23                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        159                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K9\"\n                    data-col-index=\"10\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        117                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        103                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        76                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K10\"\n                    data-col-index=\"10\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        124                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        90                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K11\"\n                    data-col-index=\"10\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        207                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        146                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J12\"\n                    data-col-index=\"9\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K12\"\n                    data-col-index=\"10\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1500                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        816                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        72                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        53                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I13\"\n                    data-col-index=\"8\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        37                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J13\"\n                    data-col-index=\"9\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K13\"\n                    data-col-index=\"10\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        86                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I14\"\n                    data-col-index=\"8\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J14\"\n                    data-col-index=\"9\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K14\"\n                    data-col-index=\"10\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        141                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        103                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I15\"\n                    data-col-index=\"8\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        72                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J15\"\n                    data-col-index=\"9\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K15\"\n                    data-col-index=\"10\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        35                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I16\"\n                    data-col-index=\"8\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J16\"\n                    data-col-index=\"9\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K16\"\n                    data-col-index=\"10\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H17\"\n                    data-col-index=\"7\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I17\"\n                    data-col-index=\"8\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J17\"\n                    data-col-index=\"9\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K17\"\n                    data-col-index=\"10\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F18\"\n                    data-col-index=\"5\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G18\"\n                    data-col-index=\"6\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        69                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H18\"\n                    data-col-index=\"7\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I18\"\n                    data-col-index=\"8\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J18\"\n                    data-col-index=\"9\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K18\"\n                    data-col-index=\"10\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        29                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A19\"\n                    data-col-index=\"0\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1700                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B19\"\n                    data-col-index=\"1\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        927                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C19\"\n                    data-col-index=\"2\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        35                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F19\"\n                    data-col-index=\"5\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G19\"\n                    data-col-index=\"6\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H19\"\n                    data-col-index=\"7\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I19\"\n                    data-col-index=\"8\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J19\"\n                    data-col-index=\"9\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K19\"\n                    data-col-index=\"10\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F20\"\n                    data-col-index=\"5\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G20\"\n                    data-col-index=\"6\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H20\"\n                    data-col-index=\"7\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I20\"\n                    data-col-index=\"8\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J20\"\n                    data-col-index=\"9\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.1*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K20\"\n                    data-col-index=\"10\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.2*                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C21\"\n                    data-col-index=\"2\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D21\"\n                    data-col-index=\"3\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E21\"\n                    data-col-index=\"4\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        69                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F21\"\n                    data-col-index=\"5\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G21\"\n                    data-col-index=\"6\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H21\"\n                    data-col-index=\"7\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I21\"\n                    data-col-index=\"8\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J21\"\n                    data-col-index=\"9\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K21\"\n                    data-col-index=\"10\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A22\"\n                    data-col-index=\"0\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B22\"\n                    data-col-index=\"1\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        982                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C22\"\n                    data-col-index=\"2\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D22\"\n                    data-col-index=\"3\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E22\"\n                    data-col-index=\"4\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F22\"\n                    data-col-index=\"5\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G22\"\n                    data-col-index=\"6\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H22\"\n                    data-col-index=\"7\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.48                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I22\"\n                    data-col-index=\"8\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J22\"\n                    data-col-index=\"9\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K22\"\n                    data-col-index=\"10\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C23\"\n                    data-col-index=\"2\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D23\"\n                    data-col-index=\"3\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E23\"\n                    data-col-index=\"4\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F23\"\n                    data-col-index=\"5\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G23\"\n                    data-col-index=\"6\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H23\"\n                    data-col-index=\"7\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I23\"\n                    data-col-index=\"8\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J23\"\n                    data-col-index=\"9\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.33*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K23\"\n                    data-col-index=\"10\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.3*                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C24\"\n                    data-col-index=\"2\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D24\"\n                    data-col-index=\"3\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E24\"\n                    data-col-index=\"4\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F24\"\n                    data-col-index=\"5\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G24\"\n                    data-col-index=\"6\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H24\"\n                    data-col-index=\"7\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I24\"\n                    data-col-index=\"8\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J24\"\n                    data-col-index=\"9\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K24\"\n                    data-col-index=\"10\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.3                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A25\"\n                    data-col-index=\"0\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1900                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B25\"\n                    data-col-index=\"1\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1038                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C25\"\n                    data-col-index=\"2\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D25\"\n                    data-col-index=\"3\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E25\"\n                    data-col-index=\"4\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F25\"\n                    data-col-index=\"5\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G25\"\n                    data-col-index=\"6\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H25\"\n                    data-col-index=\"7\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I25\"\n                    data-col-index=\"8\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J25\"\n                    data-col-index=\"9\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K25\"\n                    data-col-index=\"10\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C26\"\n                    data-col-index=\"2\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D26\"\n                    data-col-index=\"3\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E26\"\n                    data-col-index=\"4\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F26\"\n                    data-col-index=\"5\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G26\"\n                    data-col-index=\"6\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H26\"\n                    data-col-index=\"7\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.33*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I26\"\n                    data-col-index=\"8\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.3*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J26\"\n                    data-col-index=\"9\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K26\"\n                    data-col-index=\"10\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C27\"\n                    data-col-index=\"2\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D27\"\n                    data-col-index=\"3\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E27\"\n                    data-col-index=\"4\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F27\"\n                    data-col-index=\"5\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G27\"\n                    data-col-index=\"6\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H27\"\n                    data-col-index=\"7\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I27\"\n                    data-col-index=\"8\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J27\"\n                    data-col-index=\"9\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K27\"\n                    data-col-index=\"10\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A28\"\n                    data-col-index=\"0\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B28\"\n                    data-col-index=\"1\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1093                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C28\"\n                    data-col-index=\"2\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D28\"\n                    data-col-index=\"3\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.62                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E28\"\n                    data-col-index=\"4\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F28\"\n                    data-col-index=\"5\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G28\"\n                    data-col-index=\"6\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H28\"\n                    data-col-index=\"7\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I28\"\n                    data-col-index=\"8\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J28\"\n                    data-col-index=\"9\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K28\"\n                    data-col-index=\"10\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C29\"\n                    data-col-index=\"2\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D29\"\n                    data-col-index=\"3\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E29\"\n                    data-col-index=\"4\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F29\"\n                    data-col-index=\"5\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.35                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G29\"\n                    data-col-index=\"6\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H29\"\n                    data-col-index=\"7\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I29\"\n                    data-col-index=\"8\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.69*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J29\"\n                    data-col-index=\"9\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K29\"\n                    data-col-index=\"10\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C30\"\n                    data-col-index=\"2\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        R                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D30\"\n                    data-col-index=\"3\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E30\"\n                    data-col-index=\"4\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F30\"\n                    data-col-index=\"5\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G30\"\n                    data-col-index=\"6\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H30\"\n                    data-col-index=\"7\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I30\"\n                    data-col-index=\"8\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J30\"\n                    data-col-index=\"9\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K30\"\n                    data-col-index=\"10\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-547'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Significant extrapolation<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-tensile-properties\">Tensile Properties<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-tensile-data-plate\">Tensile Data, Plate<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-555\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"7\"\n           data-rows=\"9\"\n           data-wpID=\"555\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:28.571428571429%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:28.571428571429%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:28.571428571429%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate Tensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:14.285714285714%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        340                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        110.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        48.9                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        32.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        224                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        87.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        604                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60.2                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        212                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        558                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63.5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        31.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        218                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        421                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        74.5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        27.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        189                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        37.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        255                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        98.1                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        982                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        94                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        138                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        98.1                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1093                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        72                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        95.3                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-555'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-tensile-data-sheet\">Tensile Data, Sheet<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-556\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"7\"\n           data-rows=\"9\"\n           data-wpID=\"556\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:28.571428571429%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:28.571428571429%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:28.571428571429%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate Tensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:14.285714285714%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        376                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        113.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        783                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46.5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        36.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        253                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        91.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        628                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        53.6                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        34.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        241                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        84.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        580                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65.5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        33.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        233                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        424                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        95.6                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        193                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        36.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        251                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        117.9                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        982                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        88                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        130                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        81.5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1093                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50.6                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-556'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-average-effect-of-cryogenic-temperatures-on-tensile-properties\">Average Effect of Cryogenic Temperatures on Tensile Properties<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-557\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"9\"\n           data-rows=\"5\"\n           data-wpID=\"557\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:8.8967971530249%;                    padding:10px;\n                    \"\n                    >\n                                        Form                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:28.825622775801%;                    padding:10px;\n                    \"\n                    >\n                                        Condition                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:17.79359430605%;                    padding:10px;\n                    \"\n                    >\n                                        Test\nTemperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:17.79359430605%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield\nStrength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:17.79359430605%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate\nTensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:8.8967971530249%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Heat-treated at  2150\u00b0F(1177\u00b0C),\nRapid Cooled                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -311                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -196                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        150.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1036                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -108                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -78                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        118.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        819                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        51                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        72                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        324                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        104.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        721                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-557'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-all-weld-metal\">All Weld Metal<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-558\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"8\"\n           data-rows=\"6\"\n           data-wpID=\"558\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate Tensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %\u00a0                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        458                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        98.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        680                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in 1 inch                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        359                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        554                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in 1.125 inches                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        339                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        76.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        526                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in 1.125 inches                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1500                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        816                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        263                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        391                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in 1.125 inches                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-558'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">RT= Room Temperature<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-average-aged-tensile-data-room-temperature\">Average Aged Tensile Data, Room Temperature*<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-559\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"9\"\n           data-rows=\"26\"\n           data-wpID=\"559\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:11.111111111111%;                    padding:10px;\n                    \"\n                    >\n                                        Form                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:22.222222222222%;                    padding:10px;\n                    \"\n                    >\n                                        Aging\nTemperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:11.111111111111%;                    padding:10px;\n                    \"\n                    >\n                                        Aging Time                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:22.222222222222%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield\nStrength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:22.222222222222%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate\nTensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:11.111111111111%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        h                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"13\"                     data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet\n0.125 in.\n(3.2mm) thick                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SHT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SHT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        381                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        114.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        788                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        57                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        421                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        125.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        862                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        35                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        76.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        525                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        143.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        991                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        78.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        542                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        147.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1020                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        78.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        148.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1020                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        450                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        137.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        945                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        23                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        64.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        443                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        134.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        928                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        423                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        131.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        903                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        59.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        409                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        126.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        869                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        53.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        369                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        123.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        848                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        340                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        117.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        813                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I13\"\n                    data-col-index=\"8\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        29                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        48.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        332                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        115.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        793                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I14\"\n                    data-col-index=\"8\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        318                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        111.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        766                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I15\"\n                    data-col-index=\"8\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        29                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"11\"                     data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate\n1\/2 in.\n(12.7mm) thick                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SHT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SHT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        341                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        109.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        758                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I16\"\n                    data-col-index=\"8\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        390                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        121.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H17\"\n                    data-col-index=\"7\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        837                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I17\"\n                    data-col-index=\"8\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        33                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        73.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F18\"\n                    data-col-index=\"5\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        506                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G18\"\n                    data-col-index=\"6\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        142.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H18\"\n                    data-col-index=\"7\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        983                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I18\"\n                    data-col-index=\"8\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        73.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F19\"\n                    data-col-index=\"5\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        503                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G19\"\n                    data-col-index=\"6\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        143.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H19\"\n                    data-col-index=\"7\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        990                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I19\"\n                    data-col-index=\"8\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B20\"\n                    data-col-index=\"1\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F20\"\n                    data-col-index=\"5\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        392                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G20\"\n                    data-col-index=\"6\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        129.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H20\"\n                    data-col-index=\"7\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        892                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I20\"\n                    data-col-index=\"8\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        23                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D21\"\n                    data-col-index=\"3\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E21\"\n                    data-col-index=\"4\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F21\"\n                    data-col-index=\"5\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        392                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G21\"\n                    data-col-index=\"6\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        129.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H21\"\n                    data-col-index=\"7\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        896                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I21\"\n                    data-col-index=\"8\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D22\"\n                    data-col-index=\"3\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E22\"\n                    data-col-index=\"4\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F22\"\n                    data-col-index=\"5\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        388                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G22\"\n                    data-col-index=\"6\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        129.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H22\"\n                    data-col-index=\"7\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        891                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I22\"\n                    data-col-index=\"8\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"B23\"\n                    data-col-index=\"1\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"C23\"\n                    data-col-index=\"2\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D23\"\n                    data-col-index=\"3\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E23\"\n                    data-col-index=\"4\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F23\"\n                    data-col-index=\"5\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        328                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G23\"\n                    data-col-index=\"6\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        119.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H23\"\n                    data-col-index=\"7\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        820                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I23\"\n                    data-col-index=\"8\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        31                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D24\"\n                    data-col-index=\"3\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E24\"\n                    data-col-index=\"4\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F24\"\n                    data-col-index=\"5\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        310                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G24\"\n                    data-col-index=\"6\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        116.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H24\"\n                    data-col-index=\"7\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        805                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I24\"\n                    data-col-index=\"8\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D25\"\n                    data-col-index=\"3\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E25\"\n                    data-col-index=\"4\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        43.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F25\"\n                    data-col-index=\"5\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        303                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G25\"\n                    data-col-index=\"6\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        113.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H25\"\n                    data-col-index=\"7\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        784                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I25\"\n                    data-col-index=\"8\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D26\"\n                    data-col-index=\"3\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E26\"\n                    data-col-index=\"4\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        42.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F26\"\n                    data-col-index=\"5\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        394                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G26\"\n                    data-col-index=\"6\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        109.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H26\"\n                    data-col-index=\"7\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        752                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I26\"\n                    data-col-index=\"8\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-559'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Test data for each form are from a single heat. SHT=Solution heat-treated (not aged).<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-physical-properties\">Physical Properties<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-552\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"5\"\n           data-rows=\"67\"\n           data-wpID=\"552\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Physical Property                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Customary Units                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Metric Units                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Density                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        72\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">0.297 lb\/in<sup>3<\/sup><\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">8.22 g\/cm<sup>3<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Melting Range                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2300 - 2470 \u00b0F                    <\/td>\n                                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1260 - 1355\u00b0C                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"21\"                     data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Electrical Resistivity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45.21 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        114.83 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45.38 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        115.27 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45.89 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        94\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        116.56 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46.31 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        149\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        117.63 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46.78 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        205\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        118.82 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47.2 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        260\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        119.88 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47.53 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        120.73 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        700\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47.93 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        371\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        121.73 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        48.23 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        427\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        122.51 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        48.61 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        483\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        123.46 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        124.46 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.38 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        594\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        125.44 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.53 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        125.81 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1300\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.61 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        705\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        126.02 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B18\"\n                    data-col-index=\"1\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.68 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        126.2 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B19\"\n                    data-col-index=\"1\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1500\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C19\"\n                    data-col-index=\"2\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.73 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        816\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        126.32 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B20\"\n                    data-col-index=\"1\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.8 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        126.5 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B21\"\n                    data-col-index=\"1\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1700\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C21\"\n                    data-col-index=\"2\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.81 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D21\"\n                    data-col-index=\"3\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        927\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E21\"\n                    data-col-index=\"4\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        126.52 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B22\"\n                    data-col-index=\"1\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C22\"\n                    data-col-index=\"2\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.67 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D22\"\n                    data-col-index=\"3\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        983\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E22\"\n                    data-col-index=\"4\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        126.17 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B23\"\n                    data-col-index=\"1\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1900\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C23\"\n                    data-col-index=\"2\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.59 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D23\"\n                    data-col-index=\"3\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1038\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E23\"\n                    data-col-index=\"4\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        125.96 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B24\"\n                    data-col-index=\"1\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C24\"\n                    data-col-index=\"2\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.57 \u00b5ohm-in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D24\"\n                    data-col-index=\"3\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1094\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E24\"\n                    data-col-index=\"4\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        125.9 \u00b5ohm-cm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"10\"                     data-cell-id=\"A25\"\n                    data-col-index=\"0\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Thermal Conductivity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B25\"\n                    data-col-index=\"1\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C25\"\n                    data-col-index=\"2\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">63 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D25\"\n                    data-col-index=\"3\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E25\"\n                    data-col-index=\"4\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.2 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B26\"\n                    data-col-index=\"1\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C26\"\n                    data-col-index=\"2\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">76 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D26\"\n                    data-col-index=\"3\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E26\"\n                    data-col-index=\"4\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.2 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B27\"\n                    data-col-index=\"1\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C27\"\n                    data-col-index=\"2\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">98 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D27\"\n                    data-col-index=\"3\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E27\"\n                    data-col-index=\"4\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14.1 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B28\"\n                    data-col-index=\"1\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C28\"\n                    data-col-index=\"2\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">144 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D28\"\n                    data-col-index=\"3\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E28\"\n                    data-col-index=\"4\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20.9 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B29\"\n                    data-col-index=\"1\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C29\"\n                    data-col-index=\"2\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">151 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D29\"\n                    data-col-index=\"3\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        650\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E29\"\n                    data-col-index=\"4\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        21.9 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B30\"\n                    data-col-index=\"1\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1300\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C30\"\n                    data-col-index=\"2\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">159 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D30\"\n                    data-col-index=\"3\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        700\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E30\"\n                    data-col-index=\"4\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22.8 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B31\"\n                    data-col-index=\"1\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C31\"\n                    data-col-index=\"2\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">166 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D31\"\n                    data-col-index=\"3\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        750\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E31\"\n                    data-col-index=\"4\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        23.8 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B32\"\n                    data-col-index=\"1\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1500\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C32\"\n                    data-col-index=\"2\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">174 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D32\"\n                    data-col-index=\"3\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E32\"\n                    data-col-index=\"4\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24.7 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B33\"\n                    data-col-index=\"1\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C33\"\n                    data-col-index=\"2\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">182 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D33\"\n                    data-col-index=\"3\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        850\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E33\"\n                    data-col-index=\"4\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25.7 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B34\"\n                    data-col-index=\"1\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1700\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C34\"\n                    data-col-index=\"2\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">189 Btu-in\/ft<sup>2<\/sup>-hr-&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D34\"\n                    data-col-index=\"3\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E34\"\n                    data-col-index=\"4\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26.7 W\/m-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"11\"                     data-cell-id=\"A35\"\n                    data-col-index=\"0\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Specific Heat                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B35\"\n                    data-col-index=\"1\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C35\"\n                    data-col-index=\"2\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.116 Btu\/lb.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D35\"\n                    data-col-index=\"3\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E35\"\n                    data-col-index=\"4\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        486 J\/kg-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B36\"\n                    data-col-index=\"1\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C36\"\n                    data-col-index=\"2\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.117 Btu\/lb.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D36\"\n                    data-col-index=\"3\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E36\"\n                    data-col-index=\"4\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        487 J\/kg-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B37\"\n                    data-col-index=\"1\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400 \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C37\"\n                    data-col-index=\"2\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.118 Btu\/lb.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D37\"\n                    data-col-index=\"3\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E37\"\n                    data-col-index=\"4\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        484 J\/kg-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B38\"\n                    data-col-index=\"1\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C38\"\n                    data-col-index=\"2\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.119 Btu\/lb.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D38\"\n                    data-col-index=\"3\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E38\"\n                    data-col-index=\"4\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        491 J\/kg-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B39\"\n                    data-col-index=\"1\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C39\"\n                    data-col-index=\"2\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.123 Btu\/lb.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D39\"\n                    data-col-index=\"3\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E39\"\n                    data-col-index=\"4\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        507 J\/kg-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B40\"\n                    data-col-index=\"1\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C40\"\n                    data-col-index=\"2\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.130 Btu\/lb.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D40\"\n                    data-col-index=\"3\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E40\"\n                    data-col-index=\"4\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        531 J\/kg-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B41\"\n                    data-col-index=\"1\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C41\"\n                    data-col-index=\"2\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.139 Btu\/lb.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D41\"\n                    data-col-index=\"3\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E41\"\n                    data-col-index=\"4\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        564 J\/kg-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B42\"\n                    data-col-index=\"1\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C42\"\n                    data-col-index=\"2\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.151 Btu\/lb.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D42\"\n                    data-col-index=\"3\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        700\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E42\"\n                    data-col-index=\"4\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        606 J\/kg-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B43\"\n                    data-col-index=\"1\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C43\"\n                    data-col-index=\"2\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.167 Btu\/lb.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D43\"\n                    data-col-index=\"3\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E43\"\n                    data-col-index=\"4\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        657 J\/kg-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B44\"\n                    data-col-index=\"1\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C44\"\n                    data-col-index=\"2\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.186 Btu\/lb.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D44\"\n                    data-col-index=\"3\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E44\"\n                    data-col-index=\"4\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        716 J\/kg-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B45\"\n                    data-col-index=\"1\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C45\"\n                    data-col-index=\"2\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.205 Btu\/lb.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D45\"\n                    data-col-index=\"3\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E45\"\n                    data-col-index=\"4\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        784 J\/kg-\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"9\"                     data-cell-id=\"A46\"\n                    data-col-index=\"0\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Mean Coefficient of\nThermal Expansion                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B46\"\n                    data-col-index=\"1\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79 - 200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C46\"\n                    data-col-index=\"2\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.7 \u00b5in\/in.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D46\"\n                    data-col-index=\"3\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26 - 100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E46\"\n                    data-col-index=\"4\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">13.9 10<sup>-6<\/sup>m\/m-&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B47\"\n                    data-col-index=\"1\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79 - 1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C47\"\n                    data-col-index=\"2\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.4 \u00b5in\/in.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D47\"\n                    data-col-index=\"3\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26 - 500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E47\"\n                    data-col-index=\"4\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">15.0 10<sup>-6<\/sup>m\/m-&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B48\"\n                    data-col-index=\"1\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79 - 1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C48\"\n                    data-col-index=\"2\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.6 \u00b5in\/in.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D48\"\n                    data-col-index=\"3\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26 - 600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E48\"\n                    data-col-index=\"4\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">15.3 10<sup>-6<\/sup>m\/m-&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B49\"\n                    data-col-index=\"1\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79 - 1350\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C49\"\n                    data-col-index=\"2\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.8 \u00b5in\/in.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D49\"\n                    data-col-index=\"3\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26 - 700\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E49\"\n                    data-col-index=\"4\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">15.7 10<sup>-6<\/sup>m\/m-&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B50\"\n                    data-col-index=\"1\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79 - 1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C50\"\n                    data-col-index=\"2\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.9 \u00b5in\/in.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D50\"\n                    data-col-index=\"3\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26 - 750\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E50\"\n                    data-col-index=\"4\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">15.9 10<sup>-6<\/sup>m\/m-&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B51\"\n                    data-col-index=\"1\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79 - 1500\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C51\"\n                    data-col-index=\"2\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.9 \u00b5in\/in.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D51\"\n                    data-col-index=\"3\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26 - 800\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E51\"\n                    data-col-index=\"4\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">16.0 10<sup>-6<\/sup>m\/m-&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B52\"\n                    data-col-index=\"1\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79 - 1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C52\"\n                    data-col-index=\"2\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.1 \u00b5in\/in.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D52\"\n                    data-col-index=\"3\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26 - 850\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E52\"\n                    data-col-index=\"4\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">16.2 10<sup>-6<\/sup>m\/m-&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B53\"\n                    data-col-index=\"1\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79 - 1650\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C53\"\n                    data-col-index=\"2\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.1 \u00b5in\/in.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D53\"\n                    data-col-index=\"3\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26 - 900\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E53\"\n                    data-col-index=\"4\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">16.4 10<sup>-6<\/sup>m\/m-&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B54\"\n                    data-col-index=\"1\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79 - 1800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C54\"\n                    data-col-index=\"2\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9.2 \u00b5in\/in.-\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D54\"\n                    data-col-index=\"3\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26 - 975\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E54\"\n                    data-col-index=\"4\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">16.6 10<sup>-6<\/sup>m\/m-&deg;C<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"10\"                     data-cell-id=\"A55\"\n                    data-col-index=\"0\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Dynamic Modulus\nof Elasticity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B55\"\n                    data-col-index=\"1\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C55\"\n                    data-col-index=\"2\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">29.8 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D55\"\n                    data-col-index=\"3\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E55\"\n                    data-col-index=\"4\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        205 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B56\"\n                    data-col-index=\"1\"\n                    data-row-index=\"55\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C56\"\n                    data-col-index=\"2\"\n                    data-row-index=\"55\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">29.4 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D56\"\n                    data-col-index=\"3\"\n                    data-row-index=\"55\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E56\"\n                    data-col-index=\"4\"\n                    data-row-index=\"55\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        202 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B57\"\n                    data-col-index=\"1\"\n                    data-row-index=\"56\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C57\"\n                    data-col-index=\"2\"\n                    data-row-index=\"56\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">28.6 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D57\"\n                    data-col-index=\"3\"\n                    data-row-index=\"56\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E57\"\n                    data-col-index=\"4\"\n                    data-row-index=\"56\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        198 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B58\"\n                    data-col-index=\"1\"\n                    data-row-index=\"57\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C58\"\n                    data-col-index=\"2\"\n                    data-row-index=\"57\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">27.8 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D58\"\n                    data-col-index=\"3\"\n                    data-row-index=\"57\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E58\"\n                    data-col-index=\"4\"\n                    data-row-index=\"57\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        192 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B59\"\n                    data-col-index=\"1\"\n                    data-row-index=\"58\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C59\"\n                    data-col-index=\"2\"\n                    data-row-index=\"58\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">26.7 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D59\"\n                    data-col-index=\"3\"\n                    data-row-index=\"58\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E59\"\n                    data-col-index=\"4\"\n                    data-row-index=\"58\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        187 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B60\"\n                    data-col-index=\"1\"\n                    data-row-index=\"59\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C60\"\n                    data-col-index=\"2\"\n                    data-row-index=\"59\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">25.8 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D60\"\n                    data-col-index=\"3\"\n                    data-row-index=\"59\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E60\"\n                    data-col-index=\"4\"\n                    data-row-index=\"59\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        180 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B61\"\n                    data-col-index=\"1\"\n                    data-row-index=\"60\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C61\"\n                    data-col-index=\"2\"\n                    data-row-index=\"60\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">24.7 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D61\"\n                    data-col-index=\"3\"\n                    data-row-index=\"60\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E61\"\n                    data-col-index=\"4\"\n                    data-row-index=\"60\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        173 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B62\"\n                    data-col-index=\"1\"\n                    data-row-index=\"61\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C62\"\n                    data-col-index=\"2\"\n                    data-row-index=\"61\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">23.3 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D62\"\n                    data-col-index=\"3\"\n                    data-row-index=\"61\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        700\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E62\"\n                    data-col-index=\"4\"\n                    data-row-index=\"61\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        165 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B63\"\n                    data-col-index=\"1\"\n                    data-row-index=\"62\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C63\"\n                    data-col-index=\"2\"\n                    data-row-index=\"62\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">22.2 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D63\"\n                    data-col-index=\"3\"\n                    data-row-index=\"62\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E63\"\n                    data-col-index=\"4\"\n                    data-row-index=\"62\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        157 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B64\"\n                    data-col-index=\"1\"\n                    data-row-index=\"63\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C64\"\n                    data-col-index=\"2\"\n                    data-row-index=\"63\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">20.4 x 10<sup>6<\/sup> psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D64\"\n                    data-col-index=\"3\"\n                    data-row-index=\"63\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E64\"\n                    data-col-index=\"4\"\n                    data-row-index=\"63\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        148 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A65\"\n                    data-col-index=\"0\"\n                    data-row-index=\"64\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Poisson's Ratio                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B65\"\n                    data-col-index=\"1\"\n                    data-row-index=\"64\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -108\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C65\"\n                    data-col-index=\"2\"\n                    data-row-index=\"64\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.328                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D65\"\n                    data-col-index=\"3\"\n                    data-row-index=\"64\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -78 \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E65\"\n                    data-col-index=\"4\"\n                    data-row-index=\"64\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.328                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B66\"\n                    data-col-index=\"1\"\n                    data-row-index=\"65\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        72\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C66\"\n                    data-col-index=\"2\"\n                    data-row-index=\"65\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.32                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D66\"\n                    data-col-index=\"3\"\n                    data-row-index=\"65\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22 \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E66\"\n                    data-col-index=\"4\"\n                    data-row-index=\"65\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.32                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A67\"\n                    data-col-index=\"0\"\n                    data-row-index=\"66\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Magnetic Permeability                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B67\"\n                    data-col-index=\"1\"\n                    data-row-index=\"66\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"3\"  rowspan=\"1\"                     data-cell-id=\"C67\"\n                    data-col-index=\"2\"\n                    data-row-index=\"66\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.002 at 200 oersteds (15,900 A\/m)                    <\/td>\n                                                                <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-552'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*RT = Room Temperature<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-hardness-and-grain-size\">Hardness and Grain Size<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-room-temperature-hardness-of-material-solution-annealed-at-2150-f\">Room Temperature Hardness of Material Solution Annealed at 2150\u00b0F<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-139\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"5\"\n           data-rows=\"4\"\n           data-wpID=\"139\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-EEEFF1\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Form                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-EEEFF1 wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Hardness, HRBW                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-EEEFF1 wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Typical ASTM Grain Size                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        86                    <\/td>\n                                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.5-6                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        87                    <\/td>\n                                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3-5                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Bar                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        88                    <\/td>\n                                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2-5                    <\/td>\n                                                    <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-139'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-EEEFF1 { color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">HRBW = Hardness Rockwell \u201cB\u201d, Tungsten Indentor.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-aged-hardness\">Aged Hardness<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-aged-hardness-at-room-temperature\">Aged Hardness at Room Temperature*<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-544\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"5\"\n           data-rows=\"31\"\n           data-wpID=\"544\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Form                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Aging Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Aging Time                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        HRBW                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        h                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"10\"                     data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SHT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SHT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        58                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"10\"                     data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SHT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SHT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        57                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        59                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        58                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B20\"\n                    data-col-index=\"1\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D21\"\n                    data-col-index=\"3\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E21\"\n                    data-col-index=\"4\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D22\"\n                    data-col-index=\"3\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E22\"\n                    data-col-index=\"4\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"9\"                     data-cell-id=\"A23\"\n                    data-col-index=\"0\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        All Weld Metal**                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B23\"\n                    data-col-index=\"1\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C23\"\n                    data-col-index=\"2\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D23\"\n                    data-col-index=\"3\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E23\"\n                    data-col-index=\"4\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        64                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D24\"\n                    data-col-index=\"3\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E24\"\n                    data-col-index=\"4\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D25\"\n                    data-col-index=\"3\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E25\"\n                    data-col-index=\"4\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B26\"\n                    data-col-index=\"1\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C26\"\n                    data-col-index=\"2\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D26\"\n                    data-col-index=\"3\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E26\"\n                    data-col-index=\"4\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D27\"\n                    data-col-index=\"3\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E27\"\n                    data-col-index=\"4\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D28\"\n                    data-col-index=\"3\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E28\"\n                    data-col-index=\"4\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B29\"\n                    data-col-index=\"1\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C29\"\n                    data-col-index=\"2\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D29\"\n                    data-col-index=\"3\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E29\"\n                    data-col-index=\"4\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D30\"\n                    data-col-index=\"3\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E30\"\n                    data-col-index=\"4\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D31\"\n                    data-col-index=\"3\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E31\"\n                    data-col-index=\"4\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-544'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">SHT=Solution heat-treated (not aged)<br>*Single tests from a single heat for each form<br>**Gas tungsten arc welded<br>HRBW = Hardness Rockwell \u201cB\u201d, Tungsten Indentor.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-formability\">Formability<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-sheet\">Sheet<\/h3>\n\n\n\n<h4 class=\"wp-block-heading\" id=\"h-hastelloy-nbsp-x-alloy-formability\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;X alloy Formability<\/h4>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n    <h3 class=\"wpdt-c\"\n        id=\"wdt-table-title-145\">HASTELLOY<sup>\u00ae<\/sup> X alloy Formability<\/h3>\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-145\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"3\"\n           data-rows=\"3\"\n           data-wpID=\"145\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-tc-FFFFFF wpdt-bc-063D71\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:25.036603221083%;                    padding:10px;\n                    \"\n                    >\n                                        Condition                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-tc-FFFFFF wpdt-bc-063D71 wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:96.632503660322%;                    padding:10px;\n                    \"\n                    >\n                                        Typical Olsen cup Depth                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in.                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEEF1\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Heat-treated at 2150\u00b0F(1177\u00b0C), Rapid Cooled                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.48                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.3                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-145'>\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-bc-EEEEF1 { background-color: #EEEEF1 !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-impact-strength\">Impact Strength<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-average-impact-strength-plate\">Average Impact Strength, Plate*<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-548\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"4\"\n           data-rows=\"3\"\n           data-wpID=\"548\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:38.732394366197%;                    padding:10px;\n                    \"\n                    >\n                                        Condition                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:17.605633802817%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:35.211267605634%;                    padding:10px;\n                    \"\n                    >\n                                        Average Charpy V-Notch Impact Strength                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ft. - lb.                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        J                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Heat-treated at 2100\u00b0F (1149\u00b0C),Water Quenched                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        103                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        140                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-548'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Average of 28 samples from multiple heats, 0.413&#8243; &#8211; 1.25&#8243; thick, tested during years 2007 &#8211; 2014.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-aged-plate\">Aged Plate*<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-549\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"5\"\n           data-rows=\"13\"\n           data-wpID=\"549\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Aging Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Aging Time                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Average Charpy V-Notch Impact Strength                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        h                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ft.-lb.                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        J                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SHT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SHT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        95                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        129                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        33                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-549'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">SHT=Solution heat-treated (not aged) &nbsp;* Average of four tests on 1\/2-in. (12.7mm) plate from a single heat.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-oxidation-resistance\">Oxidation Resistance<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-comparative-static-oxidation-data-in-flowing-air-for-1008-hours\">Comparative Static Oxidation Data in Flowing Air for 1008 Hours*<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-550\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"9\"\n           data-rows=\"8\"\n           data-wpID=\"550\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:11.111111111111%;                    padding:10px;\n                    \"\n                    >\n                                        Alloy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:44.444444444444%;                    padding:10px;\n                    \"\n                    >\n                                        1800\u00b0F (980\u00b0C)                    <\/td>\n                                                                                    <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:44.444444444444%;                    padding:10px;\n                    \"\n                    >\n                                        2000\u00b0F (1095\u00b0C)                    <\/td>\n                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Metal Loss\/Side                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Metal Loss + CIP**\/Side                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Metal Loss\/Side                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Metal Loss + CIP**\/Side                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        X                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.007                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.74                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.019                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.038                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.069                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        INCONEL<sup>\u00ae<\/sup>\u00a0600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.32                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.008                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.90                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.023                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.028                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.041                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        INCONEL<sup>\u00ae<\/sup>\u00a0601                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.53                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.033                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.031                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.32                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.008                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.72                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.018                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.083                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.12                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800H<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.024                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.024                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.046                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.137                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.19                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-550'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Cycled to room temperature once a week &nbsp; **CIP=Continuous Internal Penetration<br>INCONEL is a trademark of Inco Family of Companies<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-schematic-representation-of-metallographic-technique-used-for-elevating-oxidation-tests\">Schematic Representation of Metallographic Technique used for<br>Elevating Oxidation Tests<\/h3>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"871\" height=\"246\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-oxidstion-1.png?resize=871%2C246&#038;ssl=1\" alt=\"\" class=\"wp-image-2985\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-oxidstion-1.png?w=871&amp;ssl=1 871w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-oxidstion-1.png?resize=300%2C85&amp;ssl=1 300w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-oxidstion-1.png?resize=768%2C217&amp;ssl=1 768w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-oxidstion-1.png?resize=620%2C175&amp;ssl=1 620w\" sizes=\"(max-width: 871px) 100vw, 871px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-comparative-average-hot-corrosion-resistance\">Comparative Average Hot Corrosion Resistance*<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-551\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"9\"\n           data-rows=\"5\"\n           data-wpID=\"551\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:22.222222222222%;                    padding:10px;\n                    \"\n                    >\n                                        Test\nTemperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:11.111111111111%;                    padding:10px;\n                    \"\n                    >\n                                        Test\nPeriod                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"6\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:66.666666666667%;                    padding:10px;\n                    \"\n                    >\n                                        Total Metal Affected\/Side                    <\/td>\n                                                                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        X                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        188                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        S                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        h                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mils                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1650                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1650                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        900                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.17                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-551'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*All tests performed by exposure to the combustion products of No. 2 fuel oil (0.4 percent sulfur) and 5 ppm of sea salt. Gas velocity over samples was 13 ft.\/sec. (4m\/s). Thermal shock frequency was one\/hour.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-carburization-resistance\">Carburization Resistance<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Tests were performed in a carburizing environment with an inlet gas mixture (volume %) of 5.0% H<sub>2<\/sub>, 5.0% CO, 5.0% CH<sub>4<\/sub>&nbsp;and the balance argon. The calculated oxygen potential and carbon activity at 1800\u00b0F (980\u00b0C) were 9 x 10<sup>-22<\/sup>&nbsp;atm. and 1.0, respectively.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The results are presented in terms of the mass of carbon pickup per unit area, which was obtained from the equation M = C (W\/A) where M = the mass of carbon pickup per unit area (mg\/cm<sup>2<\/sup>), C = difference in carbon (weight fraction) before and after exposure, W = weight of the unexposed specimen (mg) and A = surface area of the specimen exposed to the test environment (cm<sup>2<\/sup>).<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-comparative-carburization-resistance-at-1800-f-980-c-for-55-hours\">Comparative Carburization Resistance at 1800\u00b0F (980\u00b0C) for 55 Hours<\/h3>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"642\" height=\"659\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-carburization.png?resize=642%2C659&#038;ssl=1\" alt=\"\" class=\"wp-image-2989\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-carburization.png?w=642&amp;ssl=1 642w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-carburization.png?resize=292%2C300&amp;ssl=1 292w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-carburization.png?resize=620%2C636&amp;ssl=1 620w\" sizes=\"(max-width: 642px) 100vw, 642px\" \/><\/figure>\n<\/div><\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-welding\">Welding<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;X alloy is readily welded by Gas Tungsten Arc Welding (GTAW), Gas Metal Arc Welding (GMAW), Shielded Metal Arc Welding (SMAW), and resistance welding techniques. Submerged Arc Welding (SAW) is not recommended as this process is characterized by high heat input to the base metal and slow cooling of the weld.&nbsp; These factors can increase weld restraint and promote cracking.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-base-metal-preparation\">Base Metal Preparation<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">The welding surface and adjacent regions should be thoroughly cleaned with an appropriate solvent prior to any welding operation.&nbsp;&nbsp; All greases, oils, cutting oils, crayon marks, machining solutions, corrosion products, paint, scale, dye penetrant solutions, and other foreign matter should be completely removed.&nbsp; It is preferable, but not necessary, that the alloy be in the solution- annealed condition when welded.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-filler-metal-selection\">Filler Metal Selection<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;X filler wire (AWS A5.14, ERNiCrMo-2) is recommended for joining X alloy by Gas Tungsten Arc or Gas Metal Arc welding.&nbsp; Coated electrodes of X alloy are also available for Shielded Metal Arc welding in non-ASME code construction.&nbsp; For dissimilar metal joining of X&nbsp; alloy to nickel-, cobalt-, or iron- base materials, X filler wire, HAYNES<sup>\u00ae<\/sup>&nbsp;556<sup>\u00ae<\/sup>&nbsp;alloy (AWS A5.9 ER3556, AMS 5831) , HASTELLOY<sup>\u00ae<\/sup>&nbsp;S alloy (AMS 5838) or HASTELLOY<sup>\u00ae<\/sup>&nbsp;W alloy (AMS 5786, 5787) welding products may all be considered, depending upon the particular case. Please&nbsp;<a href=\"https:\/\/haynesintl.com\/es\/alloys\/soldadura-y-fabricacion\/\" target=\"_blank\" rel=\"noopener\">click here<\/a>&nbsp;or the Haynes&nbsp;<a href=\"https:\/\/wsg.haynesintl.com\/SmartGuide\/MainMenu.aspx\" target=\"_blank\" rel=\"noopener\">Welding SmartGuide<\/a>&nbsp;for more information.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-preheating-interpass-temperatures-and-post-weld-heat-treatment\">Preheating, Interpass Temperatures, and Post- Weld Heat Treatment<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Preheat is not required. Preheat is generally specified as room temperature (typical shop conditions).&nbsp;&nbsp; Interpass temperature should be maintained below 200\u00b0F (93\u00b0C). Auxiliary cooling methods may be used between weld passes, as needed, providing that such methods do not introduce contaminants.&nbsp; Post-weld heat treatment is not generally required for X alloy.&nbsp; For further information, please&nbsp;<a href=\"https:\/\/haynesintl.com\/es\/alloys\/soldadura-y-fabricacion\/\" target=\"_blank\" rel=\"noopener\">click here<\/a>.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-nominal-welding-parameters\">Nominal Welding Parameters<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Details for GTAW, GMAW and SMAW welding are given&nbsp;<a href=\"https:\/\/haynesintl.com\/es\/alloys\/soldadura-y-fabricacion\/\" target=\"_blank\" rel=\"noopener\">here<\/a>. Nominal welding parameters are provided as a guide for performing typical operations and are based upon welding conditions used in our laboratories.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\" id=\"h-mechanical-properties-of-welded-material-room-temperature-hardness-of-welded-sheet\">Mechanical Properties of Welded Material<br>Room Temperature Hardness of Welded Sheet<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-560\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"3\"\n           data-rows=\"10\"\n           data-wpID=\"560\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:52.023121387283%;                    padding:10px;\n                    \"\n                    >\n                                        Weld Method                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:28.709055876686%;                    padding:10px;\n                    \"\n                    >\n                                        Test Area                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:19.267822736031%;                    padding:10px;\n                    \"\n                    >\n                                        HRBW                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Shielded Metal Arc\n(covered electrodes)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Weld Area                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        92                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Heat-Affected Zone                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Base Metal                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        91                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Gas Tungsten Arc\n(TIG)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Weld Area                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        89                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Heat-Affected Zone                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Base Metal                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        91                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Gas Metal Arc\n(MIG)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Weld Area                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        90                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Heat-Affected Zone                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Base Metal                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        91                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-560'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">Note: Sheet was solution heat-treated prior to welding. Hardness was determined at room temperature in the as-welded condition.<br>HRBW = Hardness Rockwell \u201cB\u201d, Tungsten Indentor.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-average-short-term-tensile-data-cold-reduced-and-welded-0-109-in-2-8mm-sheet\">Average Short-term Tensile Data, Cold-reduced and Welded 0.109 in. (2.8mm) Sheet<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-561\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"6\"\n           data-rows=\"8\"\n           data-wpID=\"561\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:16.666666666667%;                    padding:10px;\n                    \"\n                    >\n                                        Condition                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:16.666666666667%;                    padding:10px;\n                    \"\n                    >\n                                        Form                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:33.333333333333%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:33.333333333333%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate Tensile Strength                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        As Cold-reduced                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Reduced 5%                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        82.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        565                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        123.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        848                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Reduced 15%                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        106.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        731                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        137.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        945                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Reduced 30%                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        137.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        945                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        161.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1110                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Cold-reduced and\nWelded, As Welded                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Reduced 5%                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        68.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        469                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        114.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        792                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Reduced 15%                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        72.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        497                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        113.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        780                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Reduced 30%                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        69.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        482                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        112.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        778                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-561'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">NOTE: All cold-reduced sheet and the various weld samples were produced from material which had been solution heat-treated prior to cold reduction or welding. All data were obtained at room temperature and are the result of a limited number of tests.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-average-tensile-data-weldments\">Average Tensile Data, Weldments<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-562\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"8\"\n           data-rows=\"11\"\n           data-wpID=\"562\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        Condition                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        Weld Method                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        Material                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate Tensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        As-Welded                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Shielded Metal Arc(covered electrodes)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet,\u00a00.125 in. (3.2mm)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        381                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        110.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate, 0.250 in. (6.4mm)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        391                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        109.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        757                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate, 0.375 in. (9.5mm)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        382                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        110.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        As-Welded                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Gas Tungsten Arc (TIG)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet,\u00a00.125 in. (3.2mm)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        59.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        407                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        110.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        759                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        26                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate,\u00a00.250 in. (6.4mm)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        53.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        365                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        738                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate,\u00a00.375 in. (9.5mm)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        379                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        742                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        As-Welded                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Gas Metal Arc(MIG)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet,\u00a00.125 in. (3.2mm)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        53.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        366                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        103.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        715                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate,\u00a00.250 in. (6.4mm)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        379                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        110.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        764                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        33                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate,\u00a00.375 in. (9.5mm)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        57.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        393                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        106.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        734                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-562'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-all-weld-metal-0\">All Weld Metal<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-563\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"8\"\n           data-rows=\"6\"\n           data-wpID=\"563\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate Tensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-tc-000000 wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-tc-000000 wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-tc-000000 wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-tc-000000 wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-tc-000000 wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-tc-000000 wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-tc-000000 wpdt-bc-EEEFF1 wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        458                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        98.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        680                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in 1 inch                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        359                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        554                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in 1.125 inches                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        339                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        76.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        526                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in 1.125 inches                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1500                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        816                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        263                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        391                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        45                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in 1.125 inches                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-563'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-tc-000000 { color: #000000 !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">RT= Room Temperature<\/p>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-average-welded-and-aged-tensile-data-room-temperature\">Average Welded and Aged Tensile Data, Room Temperature*<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-564\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"9\"\n           data-rows=\"19\"\n           data-wpID=\"564\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:12.948857453754%;                    padding:10px;\n                    \"\n                    >\n                                        Form                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:21.762785636561%;                    padding:10px;\n                    \"\n                    >\n                                        Aging Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:10.881392818281%;                    padding:10px;\n                    \"\n                    >\n                                        Aging Time                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:21.762785636561%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:21.762785636561%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate\nTensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:10.881392818281%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        h                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate 1\/2 in (12.7mm)\u00a0thick                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        330                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        109.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        752                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"8\"                     data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Gas Tungsten Arc Welded Plate,\n1\/2 in. (12.7mm)\nthick                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        455                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        126.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        875                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        33                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        86.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        596                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        150.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1035                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        82.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        572                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        145.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1003                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        58.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        401                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        128.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        884                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        430                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        127.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        878                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        430                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        125.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        863                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        343                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        105.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        726                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        323                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        98.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        676                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"8\"                     data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        All Weld Metal**                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        87.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        603                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        123.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        848                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        86.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        593                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        139.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        960                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I13\"\n                    data-col-index=\"8\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        86.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        598                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        131.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        909                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I14\"\n                    data-col-index=\"8\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1400                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        760                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        432                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        113.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        783                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I15\"\n                    data-col-index=\"8\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        418                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        110.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        762                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I16\"\n                    data-col-index=\"8\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        59.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        412                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        97.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H17\"\n                    data-col-index=\"7\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        674                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I17\"\n                    data-col-index=\"8\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"B18\"\n                    data-col-index=\"1\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1600                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        871                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        48.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F18\"\n                    data-col-index=\"5\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        330                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G18\"\n                    data-col-index=\"6\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        92.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H18\"\n                    data-col-index=\"7\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        640                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I18\"\n                    data-col-index=\"8\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        9                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                    <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F19\"\n                    data-col-index=\"5\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        319                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G19\"\n                    data-col-index=\"6\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        92.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H19\"\n                    data-col-index=\"7\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        639                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I19\"\n                    data-col-index=\"8\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-564'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Test data for each form are from a single heat.<br>**Single test data.<br>Gas tungsten arc welded.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-specifications-and-codes\">Specifications and Codes<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-specifications\">Specifications<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-553\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"2\"\n           data-rows=\"11\"\n           data-wpID=\"553\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        HASTELLOY<sup>\u00ae<\/sup> X alloy\n(N06002, W86002)                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet, Plate & Strip                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        AMS 5536SB 435\/B 435P= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Billet, Rod & Bar                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        AMS 5754SB 572\/B 572B 472P= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Coated Electrodes                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SFA 5.11\/\u00a0A 5.11(ENiCrMo-2)F= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Bare Welding Rods & Wire                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SFA 5.14\/\u00a0A 5.14(ERNiCrMo-2)AMS 5798F=43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Seamless Pipe & Tube                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 622\/B 622P= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Welded Pipe & Tube                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        AMS 5588SB 619\/B 619SB 626\/B 626P= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Fittings                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 366\/B 366P= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Forgings                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        AMS 5754                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        DIN                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17742 No. 2.4665NiCr22Fe18Mo                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Others                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        NACE MR0175ISO 15156                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-553'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-codes\">Codes<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-554\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"4\"\n           data-rows=\"15\"\n           data-wpID=\"554\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:95.693779904306%;                    padding:10px;\n                    \"\n                    >\n                                        HASTELLOY<sup>\u00ae<\/sup> X alloy\n(N06002, W86002)                    <\/td>\n                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"13\"                     data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ASME                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section l                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"4\"                     data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section lll                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Class 1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">800&deg;F (427&deg;C)<sup>1<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Class 2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">800&deg;F (427&deg;C)<sup>5<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Class 3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">800&deg;F (427&deg;C)<sup>5<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Classes TC and SC                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">800&ordm;F (427&ordm;C)<sup>2<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section lV                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HF-300.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section Vlll                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Div. 1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">1650&deg;F (899&deg;C)<sup>2<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Div. 2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">900&ordm;F (482&ordm;C)<sup>6<\/sup>1650&deg;F (899&deg;C)<sup>5<\/sup>800&deg;F (427&deg;C)(Bolting)<\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section Xll                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">650&deg;F (343&deg;C)<sup>2<\/sup><\/div>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B16.5                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">1500&deg;F (816&deg;C)<sup>3<\/sup><\/div>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B16.34                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">1500&deg;F (816&deg;C)<sup>4<\/sup><\/div>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B31.1                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B31.3                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">1500&deg;F (816&deg;C)<sup>5<\/sup><\/div>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"A15\"\n                    data-col-index=\"0\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MMPDS                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"3\"  rowspan=\"1\"                     data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.3.1                    <\/td>\n                                                                <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-554'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\"><sup>1<\/sup>Plate, Sheet, Bar, welded pipe\/tube, seamless pipe\/tube<br><sup>2<\/sup>Plate, Sheet, Bar, fittings, welded pipe\/tube, seamless pipe\/tube, Bolting<br><sup>3<\/sup>Plate, Bar<br><sup>4<\/sup>Plate, Bar, seamless pipe\/tube<br><sup>5<\/sup>Welded pipe\/tube, seamless pipe\/tube<br><sup>6<\/sup>Plate, Sheet, and Rod<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-disclaimer\">Disclaimer<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Haynes International makes all reasonable efforts to ensure the accuracy and correctness of the data displayed on this site but makes no representations or warranties as to the data\u2019s accuracy, correctness or reliability. All data are for general information only and not for providing design advice. Alloy properties disclosed here are based on work conducted principally by Haynes International, Inc. and occasionally supplemented by information from the open literature and, as such, are indicative only of the results of such tests and should not be considered guaranteed maximums or minimums.&nbsp; It is the responsibility of the user to test specific alloys under actual service conditions to determine their suitability for a particular purpose.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">For specific concentrations of elements present in a particular product and a discussion of the potential health affects thereof, refer to the Safety Data Sheets supplied by Haynes International, Inc.&nbsp; All trademarks are owned by Haynes International, Inc., unless otherwise indicated.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-alloy-brochure\">Alloy Brochure<\/h2>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/x-brochure.pdf\">Download<\/a><\/div>\n<\/div>\n<\/div><\/div>\n","protected":false},"excerpt":{"rendered":"<p>Principal Features HASTELLOY<sup>\u00ae<\/sup>&nbsp;X alloy (UNS N06002 (W86002) is a nickel-chromium-iron-molybdenum alloy that possesses an exceptional combination of oxidation resistance, fabricability and high-temperature strength. It has also been found to be exceptionally resistant to stress-corrosion cracking in petrochemical applications. X alloy exhibits good ductility after prolonged exposure at temperatures of 1200, 1400, 1600\u00b0F (650, 760 and [\u2026]<\/p>\n","protected":false},"author":2,"featured_media":0,"parent":13423,"menu_order":26,"template":"","meta":{"_acf_changed":false,"_searchwp_excluded":"","inline_featured_image":false,"jetpack_seo_llms_txt_always_include":false,"footnotes":""},"class_list":["post-13496","alloys","type-alloys","status-publish","hentry"],"acf":[],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v27.8 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>HASTELLOY\u00ae X - Haynes International<\/title>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/\" \/>\n<meta property=\"og:locale\" content=\"es_ES\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"HASTELLOY\u00ae X\" \/>\n<meta property=\"og:description\" content=\"Principal Features HASTELLOY\u00ae&nbsp;X alloy (UNS N06002 (W86002) is a nickel-chromium-iron-molybdenum alloy that possesses an exceptional combination of oxidation resistance, fabricability and high-temperature strength. It has also been found to be exceptionally resistant to stress-corrosion cracking in petrochemical applications. X alloy exhibits good ductility after prolonged exposure at temperatures of 1200, 1400, 1600\u00b0F (650, 760 and [\u2026]\" \/>\n<meta property=\"og:url\" content=\"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/\" \/>\n<meta property=\"og:site_name\" content=\"Haynes International\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/HaynesInternationalInc\/\" \/>\n<meta property=\"article:modified_time\" content=\"2025-02-25T15:38:42+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-oxidstion-1.png\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:site\" content=\"@HaynesIntl\" \/>\n<meta name=\"twitter:label1\" content=\"Tiempo de lectura\" \/>\n\t<meta name=\"twitter:data1\" content=\"7 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/es\\\/alloys\\\/portafolio-de-aleaciones\\\/aleaciones-de-alta-temperatura\\\/hastelloy-x\\\/\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/es\\\/alloys\\\/portafolio-de-aleaciones\\\/aleaciones-de-alta-temperatura\\\/hastelloy-x\\\/\",\"name\":\"HASTELLOY\u00ae X - Haynes International\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/es\\\/alloys\\\/portafolio-de-aleaciones\\\/aleaciones-de-alta-temperatura\\\/hastelloy-x\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/es\\\/alloys\\\/portafolio-de-aleaciones\\\/aleaciones-de-alta-temperatura\\\/hastelloy-x\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/hastelloyx-oxidstion-1.png\",\"datePublished\":\"2024-08-06T16:16:31+00:00\",\"dateModified\":\"2025-02-25T15:38:42+00:00\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/es\\\/alloys\\\/portafolio-de-aleaciones\\\/aleaciones-de-alta-temperatura\\\/hastelloy-x\\\/#breadcrumb\"},\"inLanguage\":\"es\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/haynesintl.com\\\/es\\\/alloys\\\/portafolio-de-aleaciones\\\/aleaciones-de-alta-temperatura\\\/hastelloy-x\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/es\\\/alloys\\\/portafolio-de-aleaciones\\\/aleaciones-de-alta-temperatura\\\/hastelloy-x\\\/#primaryimage\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/hastelloyx-oxidstion-1.png\",\"contentUrl\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/hastelloyx-oxidstion-1.png\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/es\\\/alloys\\\/portafolio-de-aleaciones\\\/aleaciones-de-alta-temperatura\\\/hastelloy-x\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/es\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Portafolio de Aleaciones\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/es\\\/alloys\\\/portafolio-de-aleaciones\\\/\"},{\"@type\":\"ListItem\",\"position\":3,\"name\":\"Aleaciones de Alta Temperatura\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/es\\\/alloys\\\/portafolio-de-aleaciones\\\/aleaciones-de-alta-temperatura\\\/\"},{\"@type\":\"ListItem\",\"position\":4,\"name\":\"HASTELLOY\u00ae X\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#website\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\",\"name\":\"Haynes International\",\"description\":\"The Home of HASTELLOY\u00ae and HAYNES\u00ae high-performance alloys\",\"publisher\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"es\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#organization\",\"name\":\"Haynes International\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"es\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/07\\\/logo.webp?fit=484%2C188&ssl=1\",\"contentUrl\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/07\\\/logo.webp?fit=484%2C188&ssl=1\",\"width\":484,\"height\":188,\"caption\":\"Haynes International\"},\"image\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/HaynesInternationalInc\\\/\",\"https:\\\/\\\/x.com\\\/HaynesIntl\",\"https:\\\/\\\/www.instagram.com\\\/haynesinternational\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/company\\\/haynes-international\\\/\"]}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"HASTELLOY\u00ae X - Haynes International","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/","og_locale":"es_ES","og_type":"article","og_title":"HASTELLOY\u00ae X","og_description":"Principal Features HASTELLOY\u00ae&nbsp;X alloy (UNS N06002 (W86002) is a nickel-chromium-iron-molybdenum alloy that possesses an exceptional combination of oxidation resistance, fabricability and high-temperature strength. It has also been found to be exceptionally resistant to stress-corrosion cracking in petrochemical applications. X alloy exhibits good ductility after prolonged exposure at temperatures of 1200, 1400, 1600\u00b0F (650, 760 and [\u2026]","og_url":"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/","og_site_name":"Haynes International","article_publisher":"https:\/\/www.facebook.com\/HaynesInternationalInc\/","article_modified_time":"2025-02-25T15:38:42+00:00","og_image":[{"url":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-oxidstion-1.png","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_site":"@HaynesIntl","twitter_misc":{"Tiempo de lectura":"7 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"WebPage","@id":"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/","url":"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/","name":"HASTELLOY\u00ae X - Haynes International","isPartOf":{"@id":"https:\/\/haynesintl.com\/en\/#website"},"primaryImageOfPage":{"@id":"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/#primaryimage"},"image":{"@id":"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/#primaryimage"},"thumbnailUrl":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-oxidstion-1.png","datePublished":"2024-08-06T16:16:31+00:00","dateModified":"2025-02-25T15:38:42+00:00","breadcrumb":{"@id":"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/#breadcrumb"},"inLanguage":"es","potentialAction":[{"@type":"ReadAction","target":["https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/"]}]},{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/#primaryimage","url":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-oxidstion-1.png","contentUrl":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloyx-oxidstion-1.png"},{"@type":"BreadcrumbList","@id":"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/hastelloy-x\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/haynesintl.com\/es\/"},{"@type":"ListItem","position":2,"name":"Portafolio de Aleaciones","item":"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/"},{"@type":"ListItem","position":3,"name":"Aleaciones de Alta Temperatura","item":"https:\/\/haynesintl.com\/es\/alloys\/portafolio-de-aleaciones\/aleaciones-de-alta-temperatura\/"},{"@type":"ListItem","position":4,"name":"HASTELLOY\u00ae X"}]},{"@type":"WebSite","@id":"https:\/\/haynesintl.com\/en\/#website","url":"https:\/\/haynesintl.com\/en\/","name":"Haynes International","description":"The Home of HASTELLOY\u00ae and HAYNES\u00ae high-performance alloys","publisher":{"@id":"https:\/\/haynesintl.com\/en\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/haynesintl.com\/en\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"es"},{"@type":"Organization","@id":"https:\/\/haynesintl.com\/en\/#organization","name":"Haynes International","url":"https:\/\/haynesintl.com\/en\/","logo":{"@type":"ImageObject","inLanguage":"es","@id":"https:\/\/haynesintl.com\/en\/#\/schema\/logo\/image\/","url":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/07\/logo.webp?fit=484%2C188&ssl=1","contentUrl":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/07\/logo.webp?fit=484%2C188&ssl=1","width":484,"height":188,"caption":"Haynes International"},"image":{"@id":"https:\/\/haynesintl.com\/en\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/HaynesInternationalInc\/","https:\/\/x.com\/HaynesIntl","https:\/\/www.instagram.com\/haynesinternational\/","https:\/\/www.linkedin.com\/company\/haynes-international\/"]}]}},"jetpack_sharing_enabled":true,"_links":{"self":[{"href":"https:\/\/haynesintl.com\/es\/wp-json\/wp\/v2\/alloys\/13496","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/haynesintl.com\/es\/wp-json\/wp\/v2\/alloys"}],"about":[{"href":"https:\/\/haynesintl.com\/es\/wp-json\/wp\/v2\/types\/alloys"}],"author":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/es\/wp-json\/wp\/v2\/users\/2"}],"version-history":[{"count":1,"href":"https:\/\/haynesintl.com\/es\/wp-json\/wp\/v2\/alloys\/13496\/revisions"}],"predecessor-version":[{"id":13497,"href":"https:\/\/haynesintl.com\/es\/wp-json\/wp\/v2\/alloys\/13496\/revisions\/13497"}],"up":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/es\/wp-json\/wp\/v2\/alloys\/13423"}],"wp:attachment":[{"href":"https:\/\/haynesintl.com\/es\/wp-json\/wp\/v2\/media?parent=13496"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}