{"id":18617,"date":"2026-05-15T12:44:12","date_gmt":"2026-05-15T12:44:12","guid":{"rendered":"https:\/\/haynesintl.com\/?page_id=18617"},"modified":"2026-05-15T13:16:06","modified_gmt":"2026-05-15T13:16:06","slug":"metaltometal-sliding-wear","status":"publish","type":"page","link":"https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/","title":{"rendered":"Metal\u2010to\u2010Metal Sliding Wear"},"content":{"rendered":"\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<p class=\"wp-block-paragraph\" id=\"h-of-the-metallic-materials-cobalt-based-alloys-are-generally-regarded-as-the-most-resistant-to-sliding-wear-at-high-loads-in-the-absence-of-lubrication-under-such-conditions-a-form-of-damage-known-as-galling-is-common-this-is-thought-to-occur-by-gross-plastic-deformation-atomic-bonding-or-cold-welding-then-fracture-on-one-or-both-surfaces-leading-to-material-transfer-as-will-be-shown-test-results-confirm-that-cobalt-based-alloys-are-resistant-to-galling-moreover-they-indicate-that-the-stainless-steels-are-very-prone-to-this-form-of-damage-independent-of-their-atomic-structure\">Of the metallic materials, cobalt-based alloys are generally regarded as the most resistant to sliding wear at high loads, in the absence of lubrication. Under such conditions, a form of damage known as \u201cgalling\u201d is common; this is thought to occur by gross plastic deformation, atomic bonding (or cold welding), then fracture on one or both surfaces, leading to material transfer. As will be shown, test results confirm that cobalt-based alloys are resistant to galling. Moreover, they indicate that the stainless steels are very prone to this form of damage, independent of their atomic structure.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Galling, however, is not the only form of damage encountered in unlubricated sliding systems. At lower loads, and particularly at high relative velocities (which induce considerable heating of the metallic surfaces), oxide growth and stripping is a possibility. Under such circumstances (sometimes termed \u201coxidative\u201d wear), the characteristics of the base metal are somewhat masked. This is certainly true at temperatures in excess of about 500\u00b0C, where oxides tend to control the sliding wear process, as long as the underlying material is sufficiently supportive. At very high temperatures, very smooth oxide surfaces can be generated on sliding metallic materials; it has been surmised that these so-called \u201cglazes\u201d might involve some form of thermal transformation, or that fine oxide particulates are easily sheared and even out the contact surfaces.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The history of metal-to-metal wear testing at Haynes International (and former companies) spans 40 years. In the early years (1978 to 1986), galling and pin-on-block tests were used to evaluate and compare the characteristics of the cast and weld overlay materials (mostly cobalt- and nickel-based) in the company portfolio at that time (the hard-facing segment of the business was sold in 1986). A pin-on-disc (POD) unit, capable of elevated temperature testing, was built, but gave dubious results, and quickly fell out of favor. Some room and elevated temperature, metal-to-metal contract testing (at General Atomic, in California) was carried out in 1981 (<em>Crook and Li, 1983<\/em>), and gave clear indications of the benefit of cobalt, even though it was concerned with weld overlay (hard-facing) materials and not wrought products.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The second period of metal-to-metal testing at Haynes International coincided with the development and promotion of ULTIMET<sup>\u00ae<\/sup>\u00a0alloy, the first wrought, cobalt-based, corrosion and wear resistant material to emerge from the laboratories of Haynes, following the sale of the hard-facing business. This period was from 1989 to 1992 and involved mostly galling tests of wrought material, although other forms of ULTIMET<sup>\u00ae<\/sup>\u00a0alloy were tested, in particular weld overlays made from Haynes-produced wrought wire consumables.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Haynes International has only recently entered its third period of metal-to-metal testing, by virtue of the purchase of an ASTM G99 compliant pin-on-disc tester, plus the re-furbishing of Haynes\u2019 galling test fixtures. More importantly, Haynes International has acquired a wide-area, laser-based, 3D measurement system, to enable extremely accurate surface analyses.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The ASTM G99 compliant, pin-on-disc test and the Haynes galling test are at opposite ends of the metal-to-metal sliding wear spectrum. The pin-on-disc test simulates high speed\/low load conditions (found in many bearings and rotating seals, for example), whereas the galling test simulates low speed\/high load conditions (found during the high torque attachment and detachment of bolts, for example). In the absence of liquids, high surface temperatures can be generated during high speed\/low load, metal-to-metal sliding; these can result in debris containing oxide particles.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Galling, on the other hand, can result in seizure (due to bonding of the materials) and can generate relatively massive amounts of damage over small sliding distances (large chunks of material being transferred from one surface to the other, or released at the interface).<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">To illustrate the influence of alloy base and of strengthening mechanism on high speed\/low load sliding wear, early work at Haynes International on the ASTM G99 compliant, pin-on-disc tester has been focused on (self-coupled) HAYNES<sup>\u00ae<\/sup>\u00a025, 230<sup>\u00ae<\/sup>, and 282<sup>\u00ae<\/sup>\u00a0alloys. HAYNES<sup>\u00ae<\/sup>\u00a025 alloy is a cobalt-based alloy containing 10 wt.% nickel to adjust its transformation tendency. HAYNES<sup>\u00ae<\/sup>\u00a0230<sup>\u00ae<\/sup>\u00a0alloy is a nickel-based alloy with remarkably similar alloying additions, at similar levels. HAYNES<sup>\u00ae<\/sup>\u00a0282<sup>\u00ae<\/sup>\u00a0alloy is a gamma-prime strengthened, nickel-based material.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The extent of pin wear on the three alloys is shown in the following bar chart, which indicates that the cobalt-based, HAYNES<sup>\u00ae<\/sup>\u00a025 alloy is the most resistant of the three alloys to wear at a load of 30 N, and a linear speed of 2 m\/s.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"550\" height=\"333\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/pin-wear-at-30n-2m-s-linear-speed.tmb-ze-550-550.jpg?resize=550%2C333&#038;ssl=1\" alt=\"\" class=\"wp-image-3774\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/pin-wear-at-30n-2m-s-linear-speed.tmb-ze-550-550.jpg?w=550&amp;ssl=1 550w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/pin-wear-at-30n-2m-s-linear-speed.tmb-ze-550-550.jpg?resize=300%2C182&amp;ssl=1 300w\" sizes=\"(max-width: 550px) 100vw, 550px\" \/><\/figure>\n<\/div>\n\n\n<p class=\"wp-block-paragraph\">Gamma-prime strengthened HAYNES<sup>\u00ae<\/sup>\u00a0282<sup>\u00ae<\/sup>\u00a0alloy was found to be significantly more resistant to wear under these conditions than the solid-solution strengthened, nickel-based, HAYNES<sup>\u00ae<\/sup>\u00a0230<sup>\u00ae<\/sup>\u00a0alloy. Moreover, it was discovered that 282<sup>\u00ae<\/sup>\u00a0alloy exhibits very low coefficients of friction at loads of 10 and 20 N, whereas the coefficients of friction for 25 and 230<sup>\u00ae<\/sup>\u00a0alloys are generally independent of load in the range 10 to 30 N, as illustrated in the charts below.<\/p>\n\n\n\n<h3 id=\"h-continuous-measurements-of-coefficient-of-friction-for-haynes-nbsp-282-nbsp-alloy-at-loads-of-10-20-and-30-newtons-linear-sliding-speed-2-m-s\" class=\"wp-block-heading\">Continuous Measurements of Coefficient of Friction for HAYNES<sup>\u00ae<\/sup>\u00a0282<sup>\u00ae<\/sup>\u00a0Alloy at<br>Loads of 10, 20, and 30 Newtons (Linear Sliding Speed 2 m\/s)<\/h3>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"550\" height=\"312\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/continuous-measurements-of-coefficient-of-friction-for-haynes-282-alloy.tmb-ze-550-550.jpg?resize=550%2C312&#038;ssl=1\" alt=\"\" class=\"wp-image-3778\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/continuous-measurements-of-coefficient-of-friction-for-haynes-282-alloy.tmb-ze-550-550.jpg?w=550&amp;ssl=1 550w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/continuous-measurements-of-coefficient-of-friction-for-haynes-282-alloy.tmb-ze-550-550.jpg?resize=300%2C170&amp;ssl=1 300w\" sizes=\"(max-width: 550px) 100vw, 550px\" \/><\/figure>\n<\/div>\n\n\n<h3 id=\"h-continuous-measurements-of-coefficient-of-friction-for-haynes-nbsp-25-alloy-at-loads-of-10-20-and-30-newtons-linear-sliding-speed-2-m-s\" class=\"wp-block-heading\">Continuous Measurements of Coefficient of Friction for HAYNES<sup>\u00ae<\/sup>\u00a025 Alloy at<br>Loads of 10, 20, and 30 Newtons (Linear Sliding Speed 2 m\/s)<\/h3>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"555\" height=\"332\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/continuous-measurements-of-coefficient-of-friction-for-haynes-25-alloy.tmb-ze-555-555.jpg?resize=555%2C332&#038;ssl=1\" alt=\"\" class=\"wp-image-3782\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/continuous-measurements-of-coefficient-of-friction-for-haynes-25-alloy.tmb-ze-555-555.jpg?w=555&amp;ssl=1 555w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/continuous-measurements-of-coefficient-of-friction-for-haynes-25-alloy.tmb-ze-555-555.jpg?resize=300%2C179&amp;ssl=1 300w\" sizes=\"(max-width: 555px) 100vw, 555px\" \/><\/figure>\n<\/div>\n\n\n<h3 id=\"h-continuous-measurements-of-coefficient-of-friction-for-haynes-nbsp-230-nbsp-alloy-at-loads-of-10-20-and-30-newtons-linear-sliding-speed-2-m-s\" class=\"wp-block-heading\">Continuous Measurements of Coefficient of Friction for HAYNES<sup>\u00ae<\/sup>\u00a0230<sup>\u00ae<\/sup>\u00a0Alloy at<br>Loads of 10, 20, and 30 Newtons (Linear Sliding Speed 2 m\/s)<\/h3>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"550\" height=\"326\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/continuous-measurements-of-coefficient-of-friction-for-haynes-230-alloy.tmb-ze-550-550.jpg?resize=550%2C326&#038;ssl=1\" alt=\"\" class=\"wp-image-3786\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/continuous-measurements-of-coefficient-of-friction-for-haynes-230-alloy.tmb-ze-550-550.jpg?w=550&amp;ssl=1 550w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/continuous-measurements-of-coefficient-of-friction-for-haynes-230-alloy.tmb-ze-550-550.jpg?resize=300%2C178&amp;ssl=1 300w\" sizes=\"(max-width: 550px) 100vw, 550px\" \/><\/figure>\n<\/div>\n\n\n<p class=\"wp-block-paragraph\">The first galling test used by Haynes International was of simple design, and involved the rotation (through 360\u00b0) of a 9.5 mm diameter pin (the sliding surface being a flat section, perpendicular to the cylindrical axis) against a block of dimensions 102 mm x 102 mm x 12.7 mm, under various loads (applied using a tensile testing machine, in compression mode). The main problem with this test, apart from load variations associated with deformation and fracture events at the sliding interface and the pin-to-machine coupling, was the subjective nature of the analysis.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Analysis involved visual inspection of the sliding surface and a determination of whether or not \u201cgalling\u201d had occurred. Tests were performed at various loads, which were converted to stresses using the apparent area of contact, and a threshold stress (the lowest at which galling was observed) determined. This first test was unable to differentiate between the various wear-resistant, cobalt-based STELLITE<sup>\u00ae<\/sup>\u00a0alloys in the Company\u2019s product portfolio at that time, and scanning electron microscopy suggested that the visual inspection was revealing only the scale of the damage, i.e. surfaces purported to be free of galling exhibited the same signs of damage, only on a micro-scale.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">To remedy some of the limitations of this first test, changes were made (especially after a visit to the tribology laboratory of Armco, which was using a similar test, but using a clockwise-anticlockwise, multiple rotation technique). The most important change was to replace visual inspection with a quantitative determination of the change in peak-to- valley amplitude of the block surface, using surface profilometry. Generally, the pin and block surfaces appeared to exhibit similar changes; it was therefore deemed appropriate to analyze only the block surface, which was more amenable to profilometry (no edge drop-off). Other changes included a pin of larger diameter (15.9 mm) to accommodate a larger female cone shape on top (to hold the ball bearing used for load transfer from the tensile machine), and a 10-stroke clockwise-anticlockwise rotation technique over a 120\u00b0 arc.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">As an aside, the ASTM Standard (G98) Test Method for Galling Resistance of Materials is similar to that used by Armco, which had a strong ASTM representation. However, it requires a single revolution of the pin (which is termed a button in the standard) and a subjective judgement of threshold galling stress (which had been deemed unacceptable for ranking of the cobalt-based alloys).<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Self-coupled\/mated galling data (for many of Haynes International\u2019s current portfolio of wrought products) generated using the test introduced in 1981, and involving surface profilometry, are given in the following three figures (each corresponding to a specific load).<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"637\" height=\"388\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-1361-kg-load.png?resize=637%2C388&#038;ssl=1\" alt=\"\" class=\"wp-image-3790\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-1361-kg-load.png?w=637&amp;ssl=1 637w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-1361-kg-load.png?resize=300%2C183&amp;ssl=1 300w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-1361-kg-load.png?resize=620%2C378&amp;ssl=1 620w\" sizes=\"(max-width: 637px) 100vw, 637px\" \/><\/figure>\n<\/div>\n\n\n<p class=\"wp-block-paragraph\">*Age Hardened<br>316L, 410, and 2205 suffered total seizure (with a degree of damage exceeding 200 \u00b5m)<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"618\" height=\"375\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-2722-kg-load.png?resize=618%2C375&#038;ssl=1\" alt=\"\" class=\"wp-image-3794\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-2722-kg-load.png?w=618&amp;ssl=1 618w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-2722-kg-load.png?resize=300%2C182&amp;ssl=1 300w\" sizes=\"(max-width: 618px) 100vw, 618px\" \/><\/figure>\n<\/div>\n\n\n<p class=\"wp-block-paragraph\">*Age Hardened<br>316L, 410, and 2205 were not tested at a load of 2722 kg<br>17-4 PH was too rough to measure (with a degree of damage exceeding 200 \u00b5m)<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"612\" height=\"374\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-4082-kg-load.png?resize=612%2C374&#038;ssl=1\" alt=\"\" class=\"wp-image-3798\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-4082-kg-load.png?w=612&amp;ssl=1 612w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-4082-kg-load.png?resize=300%2C183&amp;ssl=1 300w\" sizes=\"(max-width: 612px) 100vw, 612px\" \/><\/figure>\n<\/div>\n\n\n<p class=\"wp-block-paragraph\">*Age Hardened<br>316L, 410, and 2205 were not tested at a load of 4082 kg<br>17-4 PH was too rough to measure (with a degree of damage exceeding 200 \u00b5m)<br>The values for 230<sup>\u00ae<\/sup>\u00a0and HR-120<sup>\u00ae<\/sup>\u00a0alloys exceeded 200 \u00b5m<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"600\" height=\"366\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-ultimet-alloy-vs-counterface-material343e654546ba62e18cdfff0000376e70.jpg?resize=600%2C366&#038;ssl=1\" alt=\"\" class=\"wp-image-3802\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-ultimet-alloy-vs-counterface-material343e654546ba62e18cdfff0000376e70.jpg?w=600&amp;ssl=1 600w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-ultimet-alloy-vs-counterface-material343e654546ba62e18cdfff0000376e70.jpg?resize=300%2C183&amp;ssl=1 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/figure>\n<\/div>\n\n\n<p class=\"wp-block-paragraph\">In recognition of the fact that many applications of the wear-resistant cobalt alloys involve weld overlays (of critical surfaces), the figure below depicts the effects of dilution upon the galling resistance of ULTIMET<sup>\u00ae<\/sup>\u00a0welds, as applied by the gas tungsten arc (or TIG) welding process. These data (<em>Crook, 1993<\/em>) were generated using an unusual approach, involving the manufacture of pre-mixed consumables, and their deposition onto chilled copper blocks, to create \u201call- weld-metal\u201d samples of known and homogeneous composition.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">In acknowledgement of the fact that the effects of dilution are dependent upon the type of substrate, two compositionally dissimilar materials were selected for pre-mixing with ULTIMET<sup>\u00ae<\/sup>\u00a0alloy. These were 1040 carbon steel and 316L stainless steel. With regard to the levels of dilution chosen for study (9.1% and 16.7%), these represent \u201coverlay to substrate\u201d ratios of 10:1 and 5:1 (dilution is defined as the percentage of substrate in the weld bead). Undiluted samples of ULTIMET<sup>\u00ae<\/sup>\u00a0alloy were also prepared and tested.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">To make the pre-mixed consumables (welding rods of diameter 4.8 mm), a high frequency furnace and an overhead aspiration casting system were utilized. The charge materials were forged billet (in the case of ULTIMET<sup>\u00ae<\/sup>\u00a0alloy), and cut pieces of wrought plate (in the case of carbon steel and stainless steel).<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">From these data, it is evident that dilution (at the 9.1% and 16.7% levels, which would be considered low to moderate) has little effect upon the galling resistance of ULTIMET<sup>\u00ae<\/sup>\u00a0alloy.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"600\" height=\"366\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-ultimet-alloy-vs-counterface-material343e654546ba62e18cdfff0000376e70-1.jpg?resize=600%2C366&#038;ssl=1\" alt=\"\" class=\"wp-image-3806\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-ultimet-alloy-vs-counterface-material343e654546ba62e18cdfff0000376e70-1.jpg?w=600&amp;ssl=1 600w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/degree-of-galling-damage-um-for-ultimet-alloy-vs-counterface-material343e654546ba62e18cdfff0000376e70-1.jpg?resize=300%2C183&amp;ssl=1 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/figure>\n<\/div>\n\n\n<p class=\"wp-block-paragraph\">Although the aforementioned metal-to-metal sliding tests performed at General Atomic in 1981 concerned the performance of hard-facing (not wrought) materials, they did indicate the importance of alloy base and temperature. The resulting graphs are therefore of value, and are presented below.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"408\" height=\"426\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/wear-rates-for-alloys-containing-different-co-ni-fe-levels.jpg?resize=408%2C426&#038;ssl=1\" alt=\"\" class=\"wp-image-3810\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/wear-rates-for-alloys-containing-different-co-ni-fe-levels.jpg?w=408&amp;ssl=1 408w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/wear-rates-for-alloys-containing-different-co-ni-fe-levels.jpg?resize=287%2C300&amp;ssl=1 287w\" sizes=\"(max-width: 408px) 100vw, 408px\" \/><\/figure>\n<\/div>\n\n\n<p class=\"wp-block-paragraph\">Finally, it is important to indicate the sophistication and accuracy of modern wear testing at Haynes International. Recently (<em>Krishnamurthy and Crook, 2018<\/em>), galling tests were performed to quantify the benefits of cobalt as a wear alloy base, and to study the advantages of gamma-prime strengthening (of nickel-based alloys). To accomplish this, HAYNES<sup>\u00ae<\/sup>\u00a025, 230<sup>\u00ae<\/sup>, and 282<sup>\u00ae<\/sup>\u00a0alloys were compared. The results, which were generated using the wide-area, laser-based, 3D measurement system, are shown in the following bar charts. These involved a load of 2722 kg (6000 lb) and the 1981 multi-stroke procedures.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"634\" height=\"397\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/block-scar-roughness-um-self-coupled.jpg?resize=634%2C397&#038;ssl=1\" alt=\"\" class=\"wp-image-3814\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/block-scar-roughness-um-self-coupled.jpg?w=634&amp;ssl=1 634w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/block-scar-roughness-um-self-coupled.jpg?resize=300%2C188&amp;ssl=1 300w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/block-scar-roughness-um-self-coupled.jpg?resize=620%2C388&amp;ssl=1 620w\" sizes=\"(max-width: 634px) 100vw, 634px\" \/><\/figure>\n<\/div>\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"629\" height=\"390\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/block-scar-roughness-um-316l-stainless-steel-block.jpg?resize=629%2C390&#038;ssl=1\" alt=\"\" class=\"wp-image-3818\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/block-scar-roughness-um-316l-stainless-steel-block.jpg?w=629&amp;ssl=1 629w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/block-scar-roughness-um-316l-stainless-steel-block.jpg?resize=300%2C186&amp;ssl=1 300w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/block-scar-roughness-um-316l-stainless-steel-block.jpg?resize=620%2C384&amp;ssl=1 620w\" sizes=\"(max-width: 629px) 100vw, 629px\" \/><\/figure>\n<\/div>\n\n\n<p class=\"wp-block-paragraph\">The final figure, shown below, is a laser-generated image (magnified by 1500x) of the HAYNES<sup>\u00ae<\/sup>\u00a0230<sup>\u00ae<\/sup>\u00a0block scar, color-coded to indicate the heights and depths of the surface features.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"650\" height=\"384\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/laser-generated-image-of-haynes-230-block-scar.tmb-ze-650-650.jpg?resize=650%2C384&#038;ssl=1\" alt=\"\" class=\"wp-image-3822\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/laser-generated-image-of-haynes-230-block-scar.tmb-ze-650-650.jpg?w=650&amp;ssl=1 650w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/laser-generated-image-of-haynes-230-block-scar.tmb-ze-650-650.jpg?resize=300%2C177&amp;ssl=1 300w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/laser-generated-image-of-haynes-230-block-scar.tmb-ze-650-650.jpg?resize=620%2C366&amp;ssl=1 620w\" sizes=\"(max-width: 650px) 100vw, 650px\" \/><\/figure>\n<\/div><\/div><\/div>\n","protected":false},"excerpt":{"rendered":"<p>Of the metallic materials, cobalt-based alloys are generally regarded as the most resistant to sliding wear at high loads, in the absence of lubrication. Under such conditions, a form of damage known as \u201cgalling\u201d is common; this is thought to occur by gross plastic deformation, atomic bonding (or cold welding), then fracture on one or [\u2026]<\/p>\n","protected":false},"author":2,"featured_media":0,"parent":18508,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"template-pagenavigation.php","meta":{"_acf_changed":false,"_searchwp_excluded":"","inline_featured_image":false,"_wpcom_ai_launchpad_about_page":false,"_wpcom_ai_launchpad_gallery_page":false,"_wpcom_ai_launchpad_contact_page":false,"_wpcom_ai_launchpad_events_page":false,"_wpcom_ai_launchpad_video_page":false,"_wpcom_ai_launchpad_portfolio_piece":false,"_jetpack_hide_featured_image":false,"_jetpack_featured_image_duplicate_dismissed":0,"footnotes":""},"class_list":["post-18617","page","type-page","status-publish"],"acf":[],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v27.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Metal\u2010to\u2010Metal Sliding Wear - Haynes International<\/title>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/\" \/>\n<meta property=\"og:locale\" content=\"en_US\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Metal\u2010to\u2010Metal Sliding Wear\" \/>\n<meta property=\"og:description\" content=\"Of the metallic materials, cobalt-based alloys are generally regarded as the most resistant to sliding wear at high loads, in the absence of lubrication. Under such conditions, a form of damage known as \u201cgalling\u201d is common; this is thought to occur by gross plastic deformation, atomic bonding (or cold welding), then fracture on one or [\u2026]\" \/>\n<meta property=\"og:url\" content=\"https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/\" \/>\n<meta property=\"og:site_name\" content=\"Haynes International\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/HaynesInternationalInc\/\" \/>\n<meta property=\"article:modified_time\" content=\"2026-05-15T13:16:06+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/pin-wear-at-30n-2m-s-linear-speed.tmb-ze-550-550.jpg\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:site\" content=\"@HaynesIntl\" \/>\n<meta name=\"twitter:label1\" content=\"Est. reading time\" \/>\n\t<meta name=\"twitter:data1\" content=\"11 minutes\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/corrosion-guide\\\/metaltometal-sliding-wear\\\/\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/corrosion-guide\\\/metaltometal-sliding-wear\\\/\",\"name\":\"Metal\u2010to\u2010Metal Sliding Wear - Haynes International\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/corrosion-guide\\\/metaltometal-sliding-wear\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/corrosion-guide\\\/metaltometal-sliding-wear\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/pin-wear-at-30n-2m-s-linear-speed.tmb-ze-550-550.jpg\",\"datePublished\":\"2026-05-15T12:44:12+00:00\",\"dateModified\":\"2026-05-15T13:16:06+00:00\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/corrosion-guide\\\/metaltometal-sliding-wear\\\/#breadcrumb\"},\"inLanguage\":\"en-US\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/haynesintl.com\\\/en\\\/corrosion-guide\\\/metaltometal-sliding-wear\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"en-US\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/corrosion-guide\\\/metaltometal-sliding-wear\\\/#primaryimage\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/pin-wear-at-30n-2m-s-linear-speed.tmb-ze-550-550.jpg\",\"contentUrl\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/pin-wear-at-30n-2m-s-linear-speed.tmb-ze-550-550.jpg\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/corrosion-guide\\\/metaltometal-sliding-wear\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Corrosion Guide\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/corrosion-guide\\\/\"},{\"@type\":\"ListItem\",\"position\":3,\"name\":\"Metal\u2010to\u2010Metal Sliding Wear\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#website\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\",\"name\":\"Haynes International\",\"description\":\"The Home of HASTELLOY\u00ae and HAYNES\u00ae high-performance alloys\",\"publisher\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"en-US\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#organization\",\"name\":\"Haynes International\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"en-US\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/07\\\/logo.webp?fit=484%2C188&ssl=1\",\"contentUrl\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/07\\\/logo.webp?fit=484%2C188&ssl=1\",\"width\":484,\"height\":188,\"caption\":\"Haynes International\"},\"image\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/HaynesInternationalInc\\\/\",\"https:\\\/\\\/x.com\\\/HaynesIntl\",\"https:\\\/\\\/www.instagram.com\\\/haynesinternational\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/company\\\/haynes-international\\\/\"]}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Metal\u2010to\u2010Metal Sliding Wear - Haynes International","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/","og_locale":"en_US","og_type":"article","og_title":"Metal\u2010to\u2010Metal Sliding Wear","og_description":"Of the metallic materials, cobalt-based alloys are generally regarded as the most resistant to sliding wear at high loads, in the absence of lubrication. Under such conditions, a form of damage known as \u201cgalling\u201d is common; this is thought to occur by gross plastic deformation, atomic bonding (or cold welding), then fracture on one or [\u2026]","og_url":"https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/","og_site_name":"Haynes International","article_publisher":"https:\/\/www.facebook.com\/HaynesInternationalInc\/","article_modified_time":"2026-05-15T13:16:06+00:00","og_image":[{"url":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/pin-wear-at-30n-2m-s-linear-speed.tmb-ze-550-550.jpg","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_site":"@HaynesIntl","twitter_misc":{"Est. reading time":"11 minutes"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"WebPage","@id":"https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/","url":"https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/","name":"Metal\u2010to\u2010Metal Sliding Wear - Haynes International","isPartOf":{"@id":"https:\/\/haynesintl.com\/en\/#website"},"primaryImageOfPage":{"@id":"https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/#primaryimage"},"image":{"@id":"https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/#primaryimage"},"thumbnailUrl":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/pin-wear-at-30n-2m-s-linear-speed.tmb-ze-550-550.jpg","datePublished":"2026-05-15T12:44:12+00:00","dateModified":"2026-05-15T13:16:06+00:00","breadcrumb":{"@id":"https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/#breadcrumb"},"inLanguage":"en-US","potentialAction":[{"@type":"ReadAction","target":["https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/"]}]},{"@type":"ImageObject","inLanguage":"en-US","@id":"https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/#primaryimage","url":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/pin-wear-at-30n-2m-s-linear-speed.tmb-ze-550-550.jpg","contentUrl":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/pin-wear-at-30n-2m-s-linear-speed.tmb-ze-550-550.jpg"},{"@type":"BreadcrumbList","@id":"https:\/\/haynesintl.com\/en\/corrosion-guide\/metaltometal-sliding-wear\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/haynesintl.com\/en\/"},{"@type":"ListItem","position":2,"name":"Corrosion Guide","item":"https:\/\/haynesintl.com\/en\/corrosion-guide\/"},{"@type":"ListItem","position":3,"name":"Metal\u2010to\u2010Metal Sliding Wear"}]},{"@type":"WebSite","@id":"https:\/\/haynesintl.com\/en\/#website","url":"https:\/\/haynesintl.com\/en\/","name":"Haynes International","description":"The Home of HASTELLOY\u00ae and HAYNES\u00ae high-performance alloys","publisher":{"@id":"https:\/\/haynesintl.com\/en\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/haynesintl.com\/en\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"en-US"},{"@type":"Organization","@id":"https:\/\/haynesintl.com\/en\/#organization","name":"Haynes International","url":"https:\/\/haynesintl.com\/en\/","logo":{"@type":"ImageObject","inLanguage":"en-US","@id":"https:\/\/haynesintl.com\/en\/#\/schema\/logo\/image\/","url":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/07\/logo.webp?fit=484%2C188&ssl=1","contentUrl":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/07\/logo.webp?fit=484%2C188&ssl=1","width":484,"height":188,"caption":"Haynes International"},"image":{"@id":"https:\/\/haynesintl.com\/en\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/HaynesInternationalInc\/","https:\/\/x.com\/HaynesIntl","https:\/\/www.instagram.com\/haynesinternational\/","https:\/\/www.linkedin.com\/company\/haynes-international\/"]}]}},"jetpack_sharing_enabled":true,"_links":{"self":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/pages\/18617","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/comments?post=18617"}],"version-history":[{"count":3,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/pages\/18617\/revisions"}],"predecessor-version":[{"id":18900,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/pages\/18617\/revisions\/18900"}],"up":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/pages\/18508"}],"wp:attachment":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/media?parent=18617"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}