{"id":1973,"date":"2024-08-06T17:06:42","date_gmt":"2024-08-06T17:06:42","guid":{"rendered":"https:\/\/haynesintl.com\/alloys\/hastelloy-c-276\/"},"modified":"2025-07-07T15:18:03","modified_gmt":"2025-07-07T15:18:03","slug":"hastelloy-c-276","status":"publish","type":"alloys","link":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/","title":{"rendered":"HASTELLOY<sup>\u00ae<\/sup> C-276"},"content":{"rendered":"\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-principal-features\">Principal Features<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;C-276 alloy (UNS N10276) was the first wrought, nickel-chromium-molybdenum material to alleviate concerns over welding (by virtue of extremely low carbon and silicon contents). As such, it was widely accepted in the chemical process and associated industries, and now has a more than 50-year-old track record of proven performance in a vast number of corrosive chemicals.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Like other nickel alloys, it is ductile, easy to form and weld, and possesses exceptional resistance to stress corrosion cracking in chloride-bearing solutions (a form of degradation to which the austenitic stainless steels are prone). With its high chromium and molybdenum contents, it is able to withstand both oxidizing and non-oxidizing acids, and exhibits outstanding resistance to pitting and crevice attack in the presence of chlorides and other halides. Furthermore, it is very resistant to sulfide stress cracking and stress corrosion cracking in sour, oilfield environments.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;C-276 alloy is available in the form of plates, sheets, strips, billets, bars, wires, pipes, tubes, and covered electrodes. Typical chemical process industry (CPI) applications include reactors, heat exchangers, and columns.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">*Please contact our\u00a0<a href=\"\/contact\/technical-support\/\" target=\"_blank\" rel=\"noopener\">technical support team<\/a>\u00a0if you have technical questions about this alloy.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-nominal-composition\">Nominal Composition<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-648\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"2\"\n           data-rows=\"12\"\n           data-wpID=\"648\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        Weight %                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Nickel                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        57 Balance                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Cobalt                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.5 max.\u00a0                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Chromium                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Molybdenum                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Iron                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Tungsten                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Manganese                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Vanadium                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.35 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Silicon                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Carbon                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Copper                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5 max.\u00a0                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-648'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-iso-corrosion-diagrams\">Iso-Corrosion Diagrams<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Each of these iso-corrosion diagrams was constructed using numerous corrosion rate values, generated at different acid concentrations and temperatures. The blue line represents those combinations of acid concentration and temperature at which a corrosion rate of 0.1 mm\/y (4 mils per year) is expected, based on laboratory tests in reagent grade acids. Below the line, rates under 0.1 mm\/y are expected. Similarly, the red line indicates the combinations of acid concentration and temperature at which a corrosion rate of 0.5 mm\/y (20 mils per year) is expected. Above the line, rates over 0.5 mm\/y are expected. Between the blue and red lines, corrosion rates are expected to fall between 0.1 and 0.5 mm\/y.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"698\" height=\"750\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrobromic-acid.jpg?resize=698%2C750&#038;ssl=1\" alt=\"\" class=\"wp-image-3160\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrobromic-acid.jpg?w=698&amp;ssl=1 698w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrobromic-acid.jpg?resize=279%2C300&amp;ssl=1 279w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrobromic-acid.jpg?resize=620%2C666&amp;ssl=1 620w\" sizes=\"(max-width: 698px) 100vw, 698px\" \/><\/figure>\n<\/div>\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"698\" height=\"750\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrochloric-acid.jpg?resize=698%2C750&#038;ssl=1\" alt=\"\" class=\"wp-image-3164\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrochloric-acid.jpg?w=698&amp;ssl=1 698w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrochloric-acid.jpg?resize=279%2C300&amp;ssl=1 279w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrochloric-acid.jpg?resize=620%2C666&amp;ssl=1 620w\" sizes=\"(max-width: 698px) 100vw, 698px\" \/><\/figure>\n<\/div>\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"698\" height=\"739\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-nitric-acid.jpg?resize=698%2C739&#038;ssl=1\" alt=\"\" class=\"wp-image-3168\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-nitric-acid.jpg?w=698&amp;ssl=1 698w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-nitric-acid.jpg?resize=283%2C300&amp;ssl=1 283w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-nitric-acid.jpg?resize=620%2C656&amp;ssl=1 620w\" sizes=\"(max-width: 698px) 100vw, 698px\" \/><\/figure>\n<\/div>\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"698\" height=\"750\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-phosphoric-acid.jpg?resize=698%2C750&#038;ssl=1\" alt=\"\" class=\"wp-image-3172\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-phosphoric-acid.jpg?w=698&amp;ssl=1 698w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-phosphoric-acid.jpg?resize=279%2C300&amp;ssl=1 279w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-phosphoric-acid.jpg?resize=620%2C666&amp;ssl=1 620w\" sizes=\"(max-width: 698px) 100vw, 698px\" \/><\/figure>\n<\/div>\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"398\" height=\"421\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-sulfuric-acid.tmb-ze-398-450.jpg?resize=398%2C421&#038;ssl=1\" alt=\"\" class=\"wp-image-3176\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-sulfuric-acid.tmb-ze-398-450.jpg?w=398&amp;ssl=1 398w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-sulfuric-acid.tmb-ze-398-450.jpg?resize=284%2C300&amp;ssl=1 284w\" sizes=\"(max-width: 398px) 100vw, 398px\" \/><\/figure>\n<\/div><\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-comparative-plots\">Comparative Plots<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">To compare the performance of HASTELLOY C-276 alloy with that of other materials, it is useful to plot the 0.1 mm\/y lines. In the following graphs, the lines for C-276 alloy are compared with those of two popular, austenitic stainless steels (316L and 254SMO), and a lower-molybdenum nickel alloy (625), in hydrochloric and sulfuric acids. At hydrochloric acid concentrations above about 5%, C-276 alloy provides a quantum improvement over the stainless steels, and offers much greater resistance to higher concentrations of both acids than alloy 625. The concentration limit of 20% hydrochloric acid is the azeotrope, beyond which high temperature corrosion tests are less reliable.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"694\" height=\"751\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrochloric-line.jpg?resize=694%2C751&#038;ssl=1\" alt=\"\" class=\"wp-image-3180\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrochloric-line.jpg?w=694&amp;ssl=1 694w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrochloric-line.jpg?resize=277%2C300&amp;ssl=1 277w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrochloric-line.jpg?resize=620%2C671&amp;ssl=1 620w\" sizes=\"(max-width: 694px) 100vw, 694px\" \/><\/figure>\n<\/div><\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-selected-corrosion-data\">Selected Corrosion Data<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-419\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"10\"\n           data-rows=\"11\"\n           data-wpID=\"419\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Conc.\nWt.%                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        50\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        75\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        125\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        150\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        175\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        225\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"J1\"\n                    data-col-index=\"9\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Boiling                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107\u00b0C                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.78                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.73                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.51                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.89                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.34                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.57                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.37                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.51                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.45                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.75                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.12                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.44                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.75                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.53                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-419'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">All corrosion rates are in millimeters per year (mm\/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.<br>Data are from Corrosion Laboratory Jobs 15-02, 27-02, and 37-02.<br>All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"465\" height=\"500\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hydrobromic-c-276.tmb-ze-500-500.jpg?resize=465%2C500&#038;ssl=1\" alt=\"\" class=\"wp-image-3184\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hydrobromic-c-276.tmb-ze-500-500.jpg?w=465&amp;ssl=1 465w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hydrobromic-c-276.tmb-ze-500-500.jpg?resize=279%2C300&amp;ssl=1 279w\" sizes=\"(max-width: 465px) 100vw, 465px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-hydrochloric-acid\">Hydrochloric Acid<\/h3>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-hydrobromic-acid\">Hydrobromic Acid<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-421\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"10\"\n           data-rows=\"15\"\n           data-wpID=\"421\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Conc.Wt.%                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        50\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        75\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        125\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        150\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        175\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        225\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"J1\"\n                    data-col-index=\"9\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Boiling                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107\u00b0C                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.33                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.70                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.57                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.26                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.89                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.86                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.42                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.34                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.57                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.67                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.37                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.92                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.37                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.68                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.72                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.34                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.31                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.75                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.63                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.31                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.53                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.94                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J12\"\n                    data-col-index=\"9\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.17                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.32                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I13\"\n                    data-col-index=\"8\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J13\"\n                    data-col-index=\"9\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A14\"\n                    data-col-index=\"0\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.33                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.54                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I14\"\n                    data-col-index=\"8\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J14\"\n                    data-col-index=\"9\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A15\"\n                    data-col-index=\"0\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.55                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I15\"\n                    data-col-index=\"8\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J15\"\n                    data-col-index=\"9\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-421'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">All corrosion rates are in millimeters per year (mm\/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.<br>Data are from Corrosion Laboratory Jobs 15-02, 27-02, and 37-02.<br>All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"500\" height=\"472\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hydrochloric-c-2766765654546ba62e18cdfff0000376e70.tmb-ze-500-500.jpg?resize=500%2C472&#038;ssl=1\" alt=\"\" class=\"wp-image-3188\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hydrochloric-c-2766765654546ba62e18cdfff0000376e70.tmb-ze-500-500.jpg?w=500&amp;ssl=1 500w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hydrochloric-c-2766765654546ba62e18cdfff0000376e70.tmb-ze-500-500.jpg?resize=300%2C283&amp;ssl=1 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-nitric-acid\">Nitric Acid<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-422\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"10\"\n           data-rows=\"10\"\n           data-wpID=\"422\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Conc.Wt.%                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        50\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        75\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        125\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        150\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        175\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        225\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"J1\"\n                    data-col-index=\"9\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Boiling                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107\u00b0C                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.26                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.66                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.17                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.41                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.52                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.38                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.88                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.42                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.65                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.51                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.42                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.82                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18.42                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.41                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.53                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        22.12                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.12                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.62                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-422'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">All corrosion rates are in millimeters per year (mm\/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.<br>Data are from Corrosion Laboratory Jobs 1-74 and 19-97.<br>All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"472\" height=\"500\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/nitric-c-276.tmb-ze-500-500.jpg?resize=472%2C500&#038;ssl=1\" alt=\"\" class=\"wp-image-3192\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/nitric-c-276.tmb-ze-500-500.jpg?w=472&amp;ssl=1 472w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/nitric-c-276.tmb-ze-500-500.jpg?resize=283%2C300&amp;ssl=1 283w\" sizes=\"(max-width: 472px) 100vw, 472px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-phosphoric-acid\">Phosphoric Acid<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-423\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"10\"\n           data-rows=\"8\"\n           data-wpID=\"423\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Conc.Wt.%                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        125\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        150\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        175\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        225\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        250\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        275\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"J1\"\n                    data-col-index=\"9\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Boiling                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        121\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        135\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        149\u00b0C                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.18                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.28                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.29                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.12                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.31                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        85                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.17                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.68                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-423'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">All corrosion rates are in millimeters per year (mm\/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.<br>Data are from Corrosion Laboratory Jobs 19-95 and 64-96.<br>All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"465\" height=\"500\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/phosphoric-c-276.tmb-ze-500-500.jpg?resize=465%2C500&#038;ssl=1\" alt=\"\" class=\"wp-image-3196\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/phosphoric-c-276.tmb-ze-500-500.jpg?w=465&amp;ssl=1 465w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/phosphoric-c-276.tmb-ze-500-500.jpg?resize=279%2C300&amp;ssl=1 279w\" sizes=\"(max-width: 465px) 100vw, 465px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-sulfuric-acid\">Sulfuric Acid<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n wdtscroll\"\n    >\n        <table id=\"wpdtSimpleTable-425\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"13\"\n           data-rows=\"17\"\n           data-wpID=\"425\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        Conc.Wt.%                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        75\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        125\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        150\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        175\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        225\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        250\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"J1\"\n                    data-col-index=\"9\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        275\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"K1\"\n                    data-col-index=\"10\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"L1\"\n                    data-col-index=\"11\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        350\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"M1\"\n                    data-col-index=\"12\"\n                    data-row-index=\"0\"\n                    style=\" width:100px;                    padding:10px;\n                    \"\n                    >\n                                        Boiling                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        121\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"J2\"\n                    data-col-index=\"9\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        135\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"K2\"\n                    data-col-index=\"10\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        149\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"L2\"\n                    data-col-index=\"11\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        177\u00b0C                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K3\"\n                    data-col-index=\"10\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L3\"\n                    data-col-index=\"11\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M3\"\n                    data-col-index=\"12\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K4\"\n                    data-col-index=\"10\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L4\"\n                    data-col-index=\"11\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M4\"\n                    data-col-index=\"12\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K5\"\n                    data-col-index=\"10\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L5\"\n                    data-col-index=\"11\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M5\"\n                    data-col-index=\"12\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K6\"\n                    data-col-index=\"10\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L6\"\n                    data-col-index=\"11\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M6\"\n                    data-col-index=\"12\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K7\"\n                    data-col-index=\"10\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L7\"\n                    data-col-index=\"11\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M7\"\n                    data-col-index=\"12\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K8\"\n                    data-col-index=\"10\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L8\"\n                    data-col-index=\"11\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M8\"\n                    data-col-index=\"12\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.18                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K9\"\n                    data-col-index=\"10\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L9\"\n                    data-col-index=\"11\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M9\"\n                    data-col-index=\"12\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.49                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.42                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K10\"\n                    data-col-index=\"10\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L10\"\n                    data-col-index=\"11\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M10\"\n                    data-col-index=\"12\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.83                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.48                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K11\"\n                    data-col-index=\"10\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L11\"\n                    data-col-index=\"11\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M11\"\n                    data-col-index=\"12\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.87                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.62                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.33                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J12\"\n                    data-col-index=\"9\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K12\"\n                    data-col-index=\"10\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L12\"\n                    data-col-index=\"11\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M12\"\n                    data-col-index=\"12\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.64                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.67                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I13\"\n                    data-col-index=\"8\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.87                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J13\"\n                    data-col-index=\"9\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K13\"\n                    data-col-index=\"10\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L13\"\n                    data-col-index=\"11\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M13\"\n                    data-col-index=\"12\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.08                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A14\"\n                    data-col-index=\"0\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I14\"\n                    data-col-index=\"8\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.68                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J14\"\n                    data-col-index=\"9\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K14\"\n                    data-col-index=\"10\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L14\"\n                    data-col-index=\"11\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M14\"\n                    data-col-index=\"12\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A15\"\n                    data-col-index=\"0\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.73                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I15\"\n                    data-col-index=\"8\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.66                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J15\"\n                    data-col-index=\"9\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K15\"\n                    data-col-index=\"10\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L15\"\n                    data-col-index=\"11\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M15\"\n                    data-col-index=\"12\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        90                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.64                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I16\"\n                    data-col-index=\"8\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.79                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J16\"\n                    data-col-index=\"9\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K16\"\n                    data-col-index=\"10\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L16\"\n                    data-col-index=\"11\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M16\"\n                    data-col-index=\"12\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A17\"\n                    data-col-index=\"0\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        96                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H17\"\n                    data-col-index=\"7\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.95                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I17\"\n                    data-col-index=\"8\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J17\"\n                    data-col-index=\"9\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K17\"\n                    data-col-index=\"10\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L17\"\n                    data-col-index=\"11\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M17\"\n                    data-col-index=\"12\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-425'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">All corrosion rates are in millimeters per year (mm\/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.<br>Data are from Corrosion Laboratory Jobs 8-95, 11-95, 18-95, 43-95, 9-96, 15-96, and 20-96.<br>All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"472\" height=\"500\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/sulfuric-c-276.tmb-ze-500-500.jpg?resize=472%2C500&#038;ssl=1\" alt=\"\" class=\"wp-image-3200\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/sulfuric-c-276.tmb-ze-500-500.jpg?w=472&amp;ssl=1 472w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/sulfuric-c-276.tmb-ze-500-500.jpg?resize=283%2C300&amp;ssl=1 283w\" sizes=\"(max-width: 472px) 100vw, 472px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-nbsp-reagent-grade-solutions-mm-y\">&nbsp;Reagent Grade Solutions, mm\/y<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-427\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"8\"\n           data-rows=\"55\"\n           data-wpID=\"427\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-tc-FFFFFF wpdt-bc-063E71 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        Chemical                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063E71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        Conc.                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063E71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063E71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        125\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063E71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        150\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063E71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        175\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063E71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063E71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:12.5%;                    padding:10px;\n                    \"\n                    >\n                                        Boiling                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bold wpdt-bc-063E71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063E71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063E71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063E71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063E71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93\u00b0C                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Acetic Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        99                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Chromic Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.53                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Formic Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        88                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Hydrobromic Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"8\"                     data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Hydrobromic Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.78                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.51                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.34                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.57                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.37                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.51                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.45                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.12                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.44                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"13\"                     data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Hydrochloric Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.33                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H17\"\n                    data-col-index=\"7\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.70                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B18\"\n                    data-col-index=\"1\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F18\"\n                    data-col-index=\"5\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G18\"\n                    data-col-index=\"6\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H18\"\n                    data-col-index=\"7\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B19\"\n                    data-col-index=\"1\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C19\"\n                    data-col-index=\"2\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F19\"\n                    data-col-index=\"5\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G19\"\n                    data-col-index=\"6\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H19\"\n                    data-col-index=\"7\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B20\"\n                    data-col-index=\"1\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F20\"\n                    data-col-index=\"5\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.42                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G20\"\n                    data-col-index=\"6\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H20\"\n                    data-col-index=\"7\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B21\"\n                    data-col-index=\"1\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C21\"\n                    data-col-index=\"2\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D21\"\n                    data-col-index=\"3\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E21\"\n                    data-col-index=\"4\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F21\"\n                    data-col-index=\"5\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.57                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G21\"\n                    data-col-index=\"6\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H21\"\n                    data-col-index=\"7\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B22\"\n                    data-col-index=\"1\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C22\"\n                    data-col-index=\"2\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D22\"\n                    data-col-index=\"3\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E22\"\n                    data-col-index=\"4\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F22\"\n                    data-col-index=\"5\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.67                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G22\"\n                    data-col-index=\"6\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H22\"\n                    data-col-index=\"7\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B23\"\n                    data-col-index=\"1\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C23\"\n                    data-col-index=\"2\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D23\"\n                    data-col-index=\"3\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E23\"\n                    data-col-index=\"4\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.37                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F23\"\n                    data-col-index=\"5\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.68                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G23\"\n                    data-col-index=\"6\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H23\"\n                    data-col-index=\"7\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B24\"\n                    data-col-index=\"1\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C24\"\n                    data-col-index=\"2\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D24\"\n                    data-col-index=\"3\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E24\"\n                    data-col-index=\"4\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.31                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F24\"\n                    data-col-index=\"5\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.75                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G24\"\n                    data-col-index=\"6\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H24\"\n                    data-col-index=\"7\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B25\"\n                    data-col-index=\"1\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C25\"\n                    data-col-index=\"2\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D25\"\n                    data-col-index=\"3\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.31                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E25\"\n                    data-col-index=\"4\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.53                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F25\"\n                    data-col-index=\"5\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.94                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G25\"\n                    data-col-index=\"6\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H25\"\n                    data-col-index=\"7\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B26\"\n                    data-col-index=\"1\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C26\"\n                    data-col-index=\"2\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.17                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D26\"\n                    data-col-index=\"3\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.32                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E26\"\n                    data-col-index=\"4\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F26\"\n                    data-col-index=\"5\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G26\"\n                    data-col-index=\"6\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H26\"\n                    data-col-index=\"7\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B27\"\n                    data-col-index=\"1\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C27\"\n                    data-col-index=\"2\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D27\"\n                    data-col-index=\"3\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.33                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E27\"\n                    data-col-index=\"4\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.54                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F27\"\n                    data-col-index=\"5\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G27\"\n                    data-col-index=\"6\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H27\"\n                    data-col-index=\"7\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B28\"\n                    data-col-index=\"1\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C28\"\n                    data-col-index=\"2\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D28\"\n                    data-col-index=\"3\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E28\"\n                    data-col-index=\"4\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.55                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F28\"\n                    data-col-index=\"5\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G28\"\n                    data-col-index=\"6\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H28\"\n                    data-col-index=\"7\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A29\"\n                    data-col-index=\"0\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Hydrofluoric Acid*                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B29\"\n                    data-col-index=\"1\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C29\"\n                    data-col-index=\"2\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D29\"\n                    data-col-index=\"3\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.34                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E29\"\n                    data-col-index=\"4\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F29\"\n                    data-col-index=\"5\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G29\"\n                    data-col-index=\"6\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H29\"\n                    data-col-index=\"7\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B30\"\n                    data-col-index=\"1\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C30\"\n                    data-col-index=\"2\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D30\"\n                    data-col-index=\"3\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.41                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E30\"\n                    data-col-index=\"4\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F30\"\n                    data-col-index=\"5\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G30\"\n                    data-col-index=\"6\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H30\"\n                    data-col-index=\"7\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B31\"\n                    data-col-index=\"1\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C31\"\n                    data-col-index=\"2\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D31\"\n                    data-col-index=\"3\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.48                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E31\"\n                    data-col-index=\"4\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F31\"\n                    data-col-index=\"5\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G31\"\n                    data-col-index=\"6\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H31\"\n                    data-col-index=\"7\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"8\"                     data-cell-id=\"A32\"\n                    data-col-index=\"0\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Nitric Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B32\"\n                    data-col-index=\"1\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C32\"\n                    data-col-index=\"2\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D32\"\n                    data-col-index=\"3\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E32\"\n                    data-col-index=\"4\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F32\"\n                    data-col-index=\"5\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G32\"\n                    data-col-index=\"6\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H32\"\n                    data-col-index=\"7\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.26                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B33\"\n                    data-col-index=\"1\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C33\"\n                    data-col-index=\"2\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D33\"\n                    data-col-index=\"3\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E33\"\n                    data-col-index=\"4\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F33\"\n                    data-col-index=\"5\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G33\"\n                    data-col-index=\"6\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H33\"\n                    data-col-index=\"7\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.66                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B34\"\n                    data-col-index=\"1\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C34\"\n                    data-col-index=\"2\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D34\"\n                    data-col-index=\"3\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E34\"\n                    data-col-index=\"4\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F34\"\n                    data-col-index=\"5\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.17                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G34\"\n                    data-col-index=\"6\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.41                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H34\"\n                    data-col-index=\"7\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B35\"\n                    data-col-index=\"1\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C35\"\n                    data-col-index=\"2\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D35\"\n                    data-col-index=\"3\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E35\"\n                    data-col-index=\"4\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F35\"\n                    data-col-index=\"5\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.38                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G35\"\n                    data-col-index=\"6\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.88                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H35\"\n                    data-col-index=\"7\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B36\"\n                    data-col-index=\"1\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C36\"\n                    data-col-index=\"2\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D36\"\n                    data-col-index=\"3\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E36\"\n                    data-col-index=\"4\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F36\"\n                    data-col-index=\"5\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.65                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G36\"\n                    data-col-index=\"6\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.51                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H36\"\n                    data-col-index=\"7\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B37\"\n                    data-col-index=\"1\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C37\"\n                    data-col-index=\"2\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D37\"\n                    data-col-index=\"3\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E37\"\n                    data-col-index=\"4\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.42                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F37\"\n                    data-col-index=\"5\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.82                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G37\"\n                    data-col-index=\"6\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H37\"\n                    data-col-index=\"7\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B38\"\n                    data-col-index=\"1\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C38\"\n                    data-col-index=\"2\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D38\"\n                    data-col-index=\"3\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E38\"\n                    data-col-index=\"4\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.41                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F38\"\n                    data-col-index=\"5\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G38\"\n                    data-col-index=\"6\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.53                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H38\"\n                    data-col-index=\"7\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B39\"\n                    data-col-index=\"1\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C39\"\n                    data-col-index=\"2\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D39\"\n                    data-col-index=\"3\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E39\"\n                    data-col-index=\"4\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F39\"\n                    data-col-index=\"5\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G39\"\n                    data-col-index=\"6\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.62                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H39\"\n                    data-col-index=\"7\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"6\"                     data-cell-id=\"A40\"\n                    data-col-index=\"0\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Phosphoric Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B40\"\n                    data-col-index=\"1\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C40\"\n                    data-col-index=\"2\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D40\"\n                    data-col-index=\"3\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E40\"\n                    data-col-index=\"4\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F40\"\n                    data-col-index=\"5\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G40\"\n                    data-col-index=\"6\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H40\"\n                    data-col-index=\"7\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B41\"\n                    data-col-index=\"1\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C41\"\n                    data-col-index=\"2\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D41\"\n                    data-col-index=\"3\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E41\"\n                    data-col-index=\"4\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F41\"\n                    data-col-index=\"5\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G41\"\n                    data-col-index=\"6\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H41\"\n                    data-col-index=\"7\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B42\"\n                    data-col-index=\"1\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C42\"\n                    data-col-index=\"2\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D42\"\n                    data-col-index=\"3\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E42\"\n                    data-col-index=\"4\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F42\"\n                    data-col-index=\"5\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G42\"\n                    data-col-index=\"6\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H42\"\n                    data-col-index=\"7\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B43\"\n                    data-col-index=\"1\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C43\"\n                    data-col-index=\"2\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D43\"\n                    data-col-index=\"3\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E43\"\n                    data-col-index=\"4\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F43\"\n                    data-col-index=\"5\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G43\"\n                    data-col-index=\"6\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H43\"\n                    data-col-index=\"7\"\n                    data-row-index=\"42\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B44\"\n                    data-col-index=\"1\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C44\"\n                    data-col-index=\"2\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D44\"\n                    data-col-index=\"3\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E44\"\n                    data-col-index=\"4\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F44\"\n                    data-col-index=\"5\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G44\"\n                    data-col-index=\"6\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H44\"\n                    data-col-index=\"7\"\n                    data-row-index=\"43\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B45\"\n                    data-col-index=\"1\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        85                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C45\"\n                    data-col-index=\"2\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D45\"\n                    data-col-index=\"3\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E45\"\n                    data-col-index=\"4\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F45\"\n                    data-col-index=\"5\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G45\"\n                    data-col-index=\"6\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H45\"\n                    data-col-index=\"7\"\n                    data-row-index=\"44\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"10\"                     data-cell-id=\"A46\"\n                    data-col-index=\"0\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sulfuric Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B46\"\n                    data-col-index=\"1\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C46\"\n                    data-col-index=\"2\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D46\"\n                    data-col-index=\"3\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E46\"\n                    data-col-index=\"4\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F46\"\n                    data-col-index=\"5\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G46\"\n                    data-col-index=\"6\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H46\"\n                    data-col-index=\"7\"\n                    data-row-index=\"45\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.18                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B47\"\n                    data-col-index=\"1\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C47\"\n                    data-col-index=\"2\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D47\"\n                    data-col-index=\"3\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E47\"\n                    data-col-index=\"4\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F47\"\n                    data-col-index=\"5\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G47\"\n                    data-col-index=\"6\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H47\"\n                    data-col-index=\"7\"\n                    data-row-index=\"46\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.49                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B48\"\n                    data-col-index=\"1\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C48\"\n                    data-col-index=\"2\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D48\"\n                    data-col-index=\"3\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E48\"\n                    data-col-index=\"4\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F48\"\n                    data-col-index=\"5\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G48\"\n                    data-col-index=\"6\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.42                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H48\"\n                    data-col-index=\"7\"\n                    data-row-index=\"47\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.83                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B49\"\n                    data-col-index=\"1\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C49\"\n                    data-col-index=\"2\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D49\"\n                    data-col-index=\"3\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E49\"\n                    data-col-index=\"4\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F49\"\n                    data-col-index=\"5\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G49\"\n                    data-col-index=\"6\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.48                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H49\"\n                    data-col-index=\"7\"\n                    data-row-index=\"48\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B50\"\n                    data-col-index=\"1\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C50\"\n                    data-col-index=\"2\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D50\"\n                    data-col-index=\"3\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E50\"\n                    data-col-index=\"4\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F50\"\n                    data-col-index=\"5\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G50\"\n                    data-col-index=\"6\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.62                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H50\"\n                    data-col-index=\"7\"\n                    data-row-index=\"49\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B51\"\n                    data-col-index=\"1\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C51\"\n                    data-col-index=\"2\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D51\"\n                    data-col-index=\"3\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E51\"\n                    data-col-index=\"4\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F51\"\n                    data-col-index=\"5\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G51\"\n                    data-col-index=\"6\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.67                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H51\"\n                    data-col-index=\"7\"\n                    data-row-index=\"50\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B52\"\n                    data-col-index=\"1\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C52\"\n                    data-col-index=\"2\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D52\"\n                    data-col-index=\"3\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E52\"\n                    data-col-index=\"4\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F52\"\n                    data-col-index=\"5\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G52\"\n                    data-col-index=\"6\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H52\"\n                    data-col-index=\"7\"\n                    data-row-index=\"51\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B53\"\n                    data-col-index=\"1\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C53\"\n                    data-col-index=\"2\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D53\"\n                    data-col-index=\"3\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E53\"\n                    data-col-index=\"4\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F53\"\n                    data-col-index=\"5\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G53\"\n                    data-col-index=\"6\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H53\"\n                    data-col-index=\"7\"\n                    data-row-index=\"52\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B54\"\n                    data-col-index=\"1\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        90                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C54\"\n                    data-col-index=\"2\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D54\"\n                    data-col-index=\"3\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E54\"\n                    data-col-index=\"4\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F54\"\n                    data-col-index=\"5\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G54\"\n                    data-col-index=\"6\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H54\"\n                    data-col-index=\"7\"\n                    data-row-index=\"53\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B55\"\n                    data-col-index=\"1\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        96                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C55\"\n                    data-col-index=\"2\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D55\"\n                    data-col-index=\"3\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E55\"\n                    data-col-index=\"4\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F55\"\n                    data-col-index=\"5\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G55\"\n                    data-col-index=\"6\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H55\"\n                    data-col-index=\"7\"\n                    data-row-index=\"54\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-427'>\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-063E71 { background-color: #063E71 !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Hydrofluoric acid can also induce internal attack of nickel alloys; these values represent only external attack.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-resistance-to-pitting-and-crevice-corrosion\">Resistance to Pitting and Crevice Corrosion<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup><sup>\u00ae<\/sup><\/sup>&nbsp;C-276 alloy exhibits high resistance to chloride-induced pitting and crevice attack, forms of corrosion to which the austenitic stainless steels are particularly prone. To assess the resistance of alloys to pitting and crevice attack, it is customary to measure their Critical Pitting Temperatures and Critical Crevice Temperatures in acidified 6 wt.% ferric chloride, in accordance with the procedures defined in ASTM Standard G 48. These values represent the lowest temperatures at which pitting and crevice attack are encountered in this solution, within 72 hours. For comparison, the values for 316L, 254SMO, 625, and C-276 alloys are as follows:<\/p>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-405\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"5\"\n           data-rows=\"6\"\n           data-wpID=\"405\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Alloy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">Critical Pitting Temperature in Acidified 6% FeCl<sub>3<\/sub><\/div>                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">Critical Crevice Temperature in Acidified 6% FeCl<sub>3<\/sub><\/div>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-tc-444444 wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444 wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444 wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444 wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316L                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        59                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        32                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        254SMO                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        140                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        86                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        212                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        104                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        C-276                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        302                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        150                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        131                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-405'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">Other chloride-bearing environments, notably Green Death (11.5% H<sub>2<\/sub>SO<sub>4<\/sub>&nbsp;+ 1.2% HCl + 1% FeCl<sub>3<\/sub>&nbsp;+ 1% CuCl<sub>2<\/sub>) and Yellow Death (4% NaCl + 0.1% Fe<sub>2<\/sub>(SO<sub>4<\/sub>)<sub>3<\/sub>&nbsp;+ 0.021M HCl), have been used to compare the resistance of various alloys to pitting and crevice attack (using tests of 24 hours duration). In Green Death, the lowest temperature at which pitting has been observed in C-276 alloy is the boiling point. In Yellow Death, C-276 alloy has not exhibited pitting, even at the maximum test temperature (150\u00b0C).The Critical Crevice Temperature of C-276 alloy in Yellow Death is 60\u00b0C.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-resistance-to-stress-corrosion-cracking\">Resistance to Stress Corrosion Cracking<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">One of the chief attributes of the nickel alloys is their resistance to chloride-induced stress corrosion cracking. A common solution for assessing the resistance of materials to this extremely destructive form of attack is boiling 45% magnesium chloride (ASTM Standard G 36), typically with stressed U-bend samples. As is evident from the following results, the two nickel alloys, C-276 and 625, are much more resistant to this form of attack than the comparative, austenitic stainless steels. The tests were stopped after 1,008 hours (six weeks).<\/p>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-407\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"2\"\n           data-rows=\"5\"\n           data-wpID=\"407\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:50%;                    padding:10px;\n                    \"\n                    >\n                                        Alloy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:50%;                    padding:10px;\n                    \"\n                    >\n                                        Time to Cracking                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316L                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2 h                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        254SMO                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24 h                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        No Cracking in 1,008 h                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        C-276                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        No Cracking in 1,008 h                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-407'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-resistance-to-seawater-crevice-corrosion\">Resistance to Seawater Crevice Corrosion<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Seawater is probably the most common aqueous salt solution. Not only is it encountered in marine transportation and offshore oil rigs, but it is also used as a coolant in coastal facilities. Listed are data generated as part of a U.S. Navy study at the LaQue Laboratories in Wrightsville Beach, North Carolina (and published by D.M. Aylor et al, Paper No. 329, CORROSION 99, NACE International, 1999). Crevice tests were performed in both still (quiescent) and flowing seawater, at 29\u00b0C, plus or minus 3\u00b0C. Two samples (A &amp; B) of each alloy were tested in still water for 180 days, and likewise in flowing water. Each sample contained two possible crevice sites.<\/p>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-408\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"5\"\n           data-rows=\"6\"\n           data-wpID=\"408\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Alloy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Quiescent                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:40%;                    padding:10px;\n                    \"\n                    >\n                                        Flowing                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00a0No. of Sites Attacked                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Maximum Depth of Attack, mm                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        No. of Sites Attacked                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Maximum Depth of Attack, mm                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316L                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:2, B:2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:1.33, B:2.27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:2, B:2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:0.48, B:0.15                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        254SMO                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:2, B:2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:0.76, B:1.73                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:2, B:2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:0.01, B:<0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:1, B:2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:0.18, B:0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:2, B:2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:<0.01, B:<0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        C-276                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:1, B:1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:0.10, B:0.13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:0, B:0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        A:0, B:0                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-408'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-corrosion-resistance-of-welds\">Corrosion Resistance of Welds<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">To assess the resistance of welds to corrosion, Haynes International has chosen to test all-weld-metal samples, taken from the quadrants of cruciform assemblies, created using multiple gas metal arc (MIG) weld passes. Predictably, the inhomogeneous nature of weld microstructures leads to higher corrosion rates (than with homogeneous, wrought products). Nevertheless, HASTELLOY<sup><sup>\u00ae<\/sup><\/sup>&nbsp;C-276 alloy exhibits excellent resistance to the key, inorganic acids, even in welded form, as shown in the following table:<\/p>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-409\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"8\"\n           data-rows=\"10\"\n           data-wpID=\"409\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:11.695906432749%;                    padding:10px;\n                    \"\n                    >\n                                        Chemical                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:14.619883040936%;                    padding:10px;\n                    \"\n                    >\n                                        Concentration                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:30.409356725146%;                    padding:10px;\n                    \"\n                    >\n                                        Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:46.783625730994%;                    padding:10px;\n                    \"\n                    >\n                                        Corrosion Rate                    <\/td>\n                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        wt.%                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Weld Metal                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Wrought Base Metal                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mpy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm\/y                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mpy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm\/y                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">H<sub>2<\/sub>SO<sub>4<\/sub><\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        150                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">H<sub>2<\/sub>SO<sub>4<\/sub><\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        150                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">H<sub>2<\/sub>SO<sub>4<\/sub><\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        150                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">H<sub>2<\/sub>SO<sub>4<\/sub><\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        90                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        150                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HCl                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        8.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.22                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.17                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HCl                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.19                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HCl                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-409'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-FFFFFF { background-color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-physical-properties\">Physical Properties<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-418\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"5\"\n           data-rows=\"30\"\n           data-wpID=\"418\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:22.330097087379%;                    padding:10px;\n                    \"\n                    >\n                                        Physical Property                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:38.834951456311%;                    padding:10px;\n                    \"\n                    >\n                                        Customary Units                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:38.834951456311%;                    padding:10px;\n                    \"\n                    >\n                                        Metric Units                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Density                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">0.321 lb\/in<sup>3<\/sup><\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">8.89 g\/cm<sup>3<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"7\"                     data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Electrical Resistivity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        48.4 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.23 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        48.7 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.24 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.0 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.25 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.5 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.26 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        49.8 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.26 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50.6 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.28 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.30 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"6\"                     data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Thermal Conductivity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">71 Btu.in\/h.ft<sup>2<\/sup>.&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.5 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">77 Btu.in\/h.ft<sup>2<\/sup>.&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.2 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">90 Btu.in\/h.ft<sup>2<\/sup>.&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.9 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">104 Btu.in\/h.ft<sup>2<\/sup>.&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14.7 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">117 Btu.in\/h.ft<sup>2<\/sup>.&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16.5 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">132 Btu.in\/h.ft<sup>2<\/sup>.&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        18.3 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"6\"                     data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Mean Coefficient of\nThermal Expansion                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75-200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.2 \u00b5in\/in.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24-100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.2 \u00b5m\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75-400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.7 \u00b5in\/in.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24-200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.0 \u00b5m\/m2.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B18\"\n                    data-col-index=\"1\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77-600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.1 \u00b5in\/in.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24-300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.7 \u00b5m\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B19\"\n                    data-col-index=\"1\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77-800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C19\"\n                    data-col-index=\"2\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.3 \u00b5in\/in.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24-400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.1 \u00b5m\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B20\"\n                    data-col-index=\"1\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77-1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.4 \u00b5in\/in.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24-500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.3 \u00b5m\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B21\"\n                    data-col-index=\"1\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77-1100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C21\"\n                    data-col-index=\"2\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.8 \u00b5in\/in.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D21\"\n                    data-col-index=\"3\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24-600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E21\"\n                    data-col-index=\"4\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.8 \u00b5m\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444\"\n                                            data-cell-id=\"A22\"\n                    data-col-index=\"0\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Magnetic Permeability                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B22\"\n                    data-col-index=\"1\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200 oersted                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C22\"\n                    data-col-index=\"2\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.0002                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D22\"\n                    data-col-index=\"3\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15.9 kA\/m                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E22\"\n                    data-col-index=\"4\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.0002                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444\"\n                                            data-cell-id=\"A23\"\n                    data-col-index=\"0\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Specific Heat                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B23\"\n                    data-col-index=\"1\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C23\"\n                    data-col-index=\"2\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.102 Btu\/lb.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D23\"\n                    data-col-index=\"3\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E23\"\n                    data-col-index=\"4\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        427 J\/kg.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"5\"                     data-cell-id=\"A24\"\n                    data-col-index=\"0\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Dynamic Modulus                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B24\"\n                    data-col-index=\"1\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C24\"\n                    data-col-index=\"2\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">29.8 x 10<sup>6<\/sup>psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D24\"\n                    data-col-index=\"3\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E24\"\n                    data-col-index=\"4\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        205 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B25\"\n                    data-col-index=\"1\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C25\"\n                    data-col-index=\"2\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">28.3 x 10<sup>6<\/sup>psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D25\"\n                    data-col-index=\"3\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E25\"\n                    data-col-index=\"4\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        195 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B26\"\n                    data-col-index=\"1\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C26\"\n                    data-col-index=\"2\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">27.3 x 10<sup>6<\/sup>psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D26\"\n                    data-col-index=\"3\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E26\"\n                    data-col-index=\"4\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        189 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B27\"\n                    data-col-index=\"1\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C27\"\n                    data-col-index=\"2\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">26.4 x 10<sup>6<\/sup>psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D27\"\n                    data-col-index=\"3\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E27\"\n                    data-col-index=\"4\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        183 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B28\"\n                    data-col-index=\"1\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C28\"\n                    data-col-index=\"2\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">25.5 x 10<sup>6<\/sup>psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D28\"\n                    data-col-index=\"3\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E28\"\n                    data-col-index=\"4\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        178 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444\"\n                                            data-cell-id=\"A29\"\n                    data-col-index=\"0\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Melting Range                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B29\"\n                    data-col-index=\"1\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2415-2500\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C29\"\n                    data-col-index=\"2\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D29\"\n                    data-col-index=\"3\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1323-1371\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E29\"\n                    data-col-index=\"4\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1 wpdt-tc-444444\"\n                                            data-cell-id=\"A30\"\n                    data-col-index=\"0\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Poisson\u2019s Ratio                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B30\"\n                    data-col-index=\"1\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C30\"\n                    data-col-index=\"2\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D30\"\n                    data-col-index=\"3\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E30\"\n                    data-col-index=\"4\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.31                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-418'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">RT = Room Temperature<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-impact-strength\">Impact Strength<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-410\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"4\"\n           data-rows=\"4\"\n           data-wpID=\"410\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:50%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:50%;                    padding:10px;\n                    \"\n                    >\n                                        Impact Strength                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-tc-444444 wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444 wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444 wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ft-lbf                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-tc-444444 wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        J                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        353                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        479                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -320                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -196                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        383                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        519                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-410'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">Impact strengths were generated using Charpy V-notch samples, machined from mill annealed plate.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-tensile-strength-and-elongation\">Tensile Strength and Elongation<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-411\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"10\"\n           data-rows=\"20\"\n           data-wpID=\"411\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Form                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Thickness                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        0.2%OffsetYield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate TensileStrength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"J1\"\n                    data-col-index=\"9\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"J2\"\n                    data-col-index=\"9\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.078                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        51.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        356                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        114.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        792                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        204                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.078                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        42.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        290                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        694                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        59                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.078                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        35.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        248                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        98.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        681                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        68                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        427                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.078                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        32.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        225                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        94.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        650                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        67                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        204                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.094                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        39.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        275                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        101.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        696                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        58                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.094                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        33.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        231                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        97.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        673                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        64                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        427                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.094                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        29.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        205                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        645                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        64                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        204                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.063-0.187                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.6-4.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        42.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        290                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        695                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.063-0.187                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.6-4.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        37.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        260                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        97.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        669                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        64                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        427                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.063-0.187                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.6-4.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        34.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        240                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        95.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        655                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J12\"\n                    data-col-index=\"9\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.063-0.187                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.6-4.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        33.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        233                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        88.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I13\"\n                    data-col-index=\"8\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        613                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J13\"\n                    data-col-index=\"9\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A14\"\n                    data-col-index=\"0\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        204                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.188-1.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.8-25.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        263                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        98.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I14\"\n                    data-col-index=\"8\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        682                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J14\"\n                    data-col-index=\"9\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A15\"\n                    data-col-index=\"0\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.188-1.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.8-25.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        34.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        235                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        94.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I15\"\n                    data-col-index=\"8\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        650                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J15\"\n                    data-col-index=\"9\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        427                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.188-1.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.8-25.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        32.7                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        225                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        91.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I16\"\n                    data-col-index=\"8\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        631                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J16\"\n                    data-col-index=\"9\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A17\"\n                    data-col-index=\"0\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.188-1.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.8-25.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        32.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        226                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H17\"\n                    data-col-index=\"7\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        87.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I17\"\n                    data-col-index=\"8\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        601                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J17\"\n                    data-col-index=\"9\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        59                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A18\"\n                    data-col-index=\"0\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B18\"\n                    data-col-index=\"1\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F18\"\n                    data-col-index=\"5\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G18\"\n                    data-col-index=\"6\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        365                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H18\"\n                    data-col-index=\"7\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        113.9                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I18\"\n                    data-col-index=\"8\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        785                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J18\"\n                    data-col-index=\"9\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        59                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A19\"\n                    data-col-index=\"0\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B19\"\n                    data-col-index=\"1\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C19\"\n                    data-col-index=\"2\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F19\"\n                    data-col-index=\"5\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        36.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G19\"\n                    data-col-index=\"6\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        250                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H19\"\n                    data-col-index=\"7\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        96.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I19\"\n                    data-col-index=\"8\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        664                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J19\"\n                    data-col-index=\"9\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A20\"\n                    data-col-index=\"0\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B20\"\n                    data-col-index=\"1\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        427                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F20\"\n                    data-col-index=\"5\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G20\"\n                    data-col-index=\"6\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        210                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H20\"\n                    data-col-index=\"7\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        94.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I20\"\n                    data-col-index=\"8\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        654                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J20\"\n                    data-col-index=\"9\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-411'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">1: Average of 25 tests<br>2: Average of 34-36 tests<br>3: Average of 9-11 tests<br>RT= Room Temperature<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-hardness\">Hardness<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-412\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"3\"\n           data-rows=\"4\"\n           data-wpID=\"412\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:33.333333333333%;                    padding:10px;\n                    \"\n                    >\n                                        Form                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:33.333333333333%;                    padding:10px;\n                    \"\n                    >\n                                        Hardness, HRBW                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:33.333333333333%;                    padding:10px;\n                    \"\n                    >\n                                        Typical ASTM Grain Size                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        88                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.5 - 6                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        88                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1 - 5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Bar                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        86                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1 - 5                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-412'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">All samples tested in solution-annealed condition.<br>HRBW = Hardness Rockwell \u201cB\u201d, Tungsten Indentor.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-welding-and-fabrication\">Welding and Fabrication<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;C-276&nbsp;alloy is very amenable to the Gas Metal Arc (GMA\/MIG), Gas Tungsten Arc (GTA\/TIG), and Shielded Metal Arc (SMA\/Stick) welding processes.&nbsp;For matching filler metals (i.e. solid wires and coated electrodes) that are available for these processes, and welding guidelines, please&nbsp;<a href=\"\/datasheet\/welding-and-fabrication\" target=\"_blank\" rel=\"noopener\">click here<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Wrought products of HASTELLOY<sup>\u00ae<\/sup>&nbsp;C-276 alloy are supplied in the Mill Annealed (MA) condition, unless otherwise specified. This solution annealing procedure has been designed to optimize the alloy\u2019s corrosion resistance and ductility. Following all hot forming operations, the material should be re-annealed, to restore optimum properties. The alloy should also be re-annealed after any cold forming operations that result in an outer fiber elongation of 7% or more. The annealing temperature for HASTELLOY<sup>\u00ae<\/sup>&nbsp;C-276 alloy is 1121\u00b0C (2050\u00b0F), and water quenching is advised (rapid air cooling is feasible with structures thinner than 10 mm (0.375 in). A hold time at the annealing temperature of 10 to 30 minutes is recommended, depending on the thickness of the structure (thicker structures need the full 30 minutes). For more details concerning the heat treatment of HASTELLOY<sup>\u00ae<\/sup>&nbsp;C-276 alloy, please&nbsp;<a href=\"\/datasheet\/welding-and-fabrication\" target=\"_blank\" rel=\"noopener\">click here<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;C-276 alloy can be hot forged, hot rolled, hot upset, hot extruded, and hot formed. However, it is more sensitive to strain and strain rates than the austenitic stainless steels, and the hot working temperature range is quite narrow. For example, the recommended start temperature for hot forging is 1232\u00b0C (2250\u00b0F) and the recommended finish temperature is 954\u00b0C (1750\u00b0F). Moderate reductions and frequent re-heating provide the best results, as described&nbsp;<a href=\"\/datasheet\/welding-and-fabrication\" target=\"_blank\" rel=\"noopener\">here<\/a>. This reference also provides guidelines for cold forming, spinning, drop hammering, punching, and shearing. The alloy is stiffer than most austenitic stainless steels, and more energy is required during cold forming. Also, HASTELLOY<sup>\u00ae<\/sup>&nbsp;C-276 alloy work hardens more readily than most austenitic stainless steels, and may require several stages of cold work, with intermediate anneals.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">While cold work does not usually affect the resistance of HASTELLOY<sup>\u00ae<\/sup>&nbsp;C-276 alloy to general corrosion, and to chloride-induced pitting and crevice attack, it can affect resistance to stress corrosion cracking. For optimum corrosion performance, therefore, the re-annealing of cold worked parts (following an outer fiber elongation of 7% or more) is important.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-specifications-and-codes\">Specifications and Codes<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-specifications\">Specifications<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-413\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"2\"\n           data-rows=\"12\"\n           data-wpID=\"413\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        HASTELLOY<sup>\u00ae<\/sup> C-276 alloy\n(N10276, W10276)                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet, Plate & Strip                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 575\/B 575P= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Billet, Rod & Bar                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 574\/B 574P= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Coated Electrodes                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SFA 5.11\/ A 5.11 (ENiCrMo-4)DIN 2.4887(EL-NiMo15Cr15W)F= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Bare Welding Rods & Wire                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SFA 5.14\/ A 5.14 (ERNiCrMo-4)DIN 2.4886(SG-NiMo16Cr16W)F= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Seamless Pipe & Tube                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 622\/B 622P= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Welded Pipe & Tube                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 619\/B 619P= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Fittings                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 366\/B 366P= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Forgings                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 564\/B 564P= 43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        DIN                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17744 No. 2.4819 NiMo16Cr15W                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        T\u00dcV                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Werkstoffblatt 400Kennblatt 320Kennblatt 319                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Others                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        NACE MR0175ISO 15156                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-413'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-codes\">Codes<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-414\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"4\"\n           data-rows=\"13\"\n           data-wpID=\"414\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-bold wpdt-tc-FFFFFF wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        HASTELLOY<sup>\u00ae<\/sup> C-276 alloy\n(N10276, W10276)                    <\/td>\n                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-tc-444444 wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"11\"                     data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ASME                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section l                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">1000&deg;F (538&deg;C)<sup>1<\/sup><\/div>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section lll                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Class 1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Class 2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">800&deg;F (427&deg;C)<sup>2<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Class 3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">800&deg;F (427&deg;C)<sup>2<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section Vlll                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Div. 1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">1250&deg;F (677&deg;C)<sup>3<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Div. 2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">1250&deg;F (677&deg;C)<sup>3<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section Xll                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">650&deg;F (343&deg;C)<sup>3<\/sup><\/div>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B16.5                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">1250&deg;F (677&deg;C)<sup>4<\/sup><\/div>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B16.34                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">1250&deg;F (677&deg;C)<sup>5<\/sup><\/div>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B31.1                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">1000&deg;F (538&deg;C)<sup>6<\/sup><\/div>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B31.3                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">1250&deg;F (677&deg;C)<sup>7<\/sup><\/div>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-tc-444444 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        VdT\u00dcV (doc #)                    <\/td>\n                                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        844\u00b0F (450\u00b0C)8,#400                    <\/td>\n                                                    <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-414'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\"><sup>1<\/sup>Plate, Sheet, Bar, fittings, welded pipe\/tube, seamless pipe\/tube<br><sup>2<\/sup>Plate, Sheet, Bar, welded pipe\/tube, seamless pipe\/tube<br><sup>3<\/sup>Plate, Sheet, Bar, Forgings, fittings, welded pipe\/tube, seamless pipe\/tube<br><sup>4<\/sup>Plate, Forgings, fittings<br><sup>5<\/sup>Plate, Bar, Forgings, seamless pipe\/tube<br><sup>6<\/sup>Plate, Sheet, fittings, welded pipe\/tube, seamless pipe\/tube<br><sup>7<\/sup>Plate, Sheet, Forgings, fittings, welded pipe\/tube, seamless pipe\/tube<br><sup>8<\/sup>Plate, Sheet, Bar, Forgings<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-disclaimer\">Disclaimer<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Haynes International makes all reasonable efforts to ensure the accuracy and correctness of the data displayed on this site but makes no representations or warranties as to the data\u2019s accuracy, correctness or reliability. All data are for general information only and not for providing design advice. Alloy properties disclosed here are based on work conducted principally by Haynes International, Inc. and occasionally supplemented by information from the open literature and, as such, are indicative only of the results of such tests and should not be considered guaranteed maximums or minimums.&nbsp; It is the responsibility of the user to test specific alloys under actual service conditions to determine their suitability for a particular purpose.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">For specific concentrations of elements present in a particular product and a discussion of the potential health affects thereof, refer to the Safety Data Sheets supplied by Haynes International, Inc.&nbsp; All trademarks are owned by Haynes International, Inc., unless otherwise indicated.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-alloy-brochure\">Alloy Brochure<\/h2>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276.pdf\">Download<\/a><\/div>\n<\/div>\n<\/div><\/div>\n","protected":false},"excerpt":{"rendered":"<p>Principal Features HASTELLOY<sup>\u00ae<\/sup>&nbsp;C-276 alloy (UNS N10276) was the first wrought, nickel-chromium-molybdenum material to alleviate concerns over welding (by virtue of extremely low carbon and silicon contents). As such, it was widely accepted in the chemical process and associated industries, and now has a more than 50-year-old track record of proven performance in a vast number [\u2026]<\/p>\n","protected":false},"author":2,"featured_media":0,"parent":29,"menu_order":4,"template":"","meta":{"_acf_changed":false,"_searchwp_excluded":"","inline_featured_image":false,"footnotes":""},"class_list":["post-1973","alloys","type-alloys","status-publish","hentry"],"acf":[],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v27.8 (Yoast SEO v28.7) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>HASTELLOY\u00ae C-276 - Haynes International<\/title>\n<meta name=\"description\" content=\"Discover HAYNES\u00aeC-276 alloy, a nickel-chromium-molybdenum superalloy renowned for its outstanding resistance to pitting, crevice corrosion, and stress corrosion cracking in both oxidizing and reducing environments. Ideal for critical chemical processing, pollution control, and harsh industrial applications.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/\" \/>\n<meta property=\"og:locale\" content=\"en_US\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"HASTELLOY\u00ae C-276\" \/>\n<meta property=\"og:description\" content=\"Discover HAYNES\u00aeC-276 alloy, a nickel-chromium-molybdenum superalloy renowned for its outstanding resistance to pitting, crevice corrosion, and stress corrosion cracking in both oxidizing and reducing environments. Ideal for critical chemical processing, pollution control, and harsh industrial applications.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/\" \/>\n<meta property=\"og:site_name\" content=\"Haynes International\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/HaynesInternationalInc\/\" \/>\n<meta property=\"article:modified_time\" content=\"2025-07-07T15:18:03+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrobromic-acid.jpg\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:site\" content=\"@HaynesIntl\" \/>\n<meta name=\"twitter:label1\" content=\"Est. reading time\" \/>\n\t<meta name=\"twitter:data1\" content=\"11 minutes\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-c-276\\\/\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-c-276\\\/\",\"name\":\"HASTELLOY\u00ae C-276 - Haynes International\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-c-276\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-c-276\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/c-276-alloy-hydrobromic-acid.jpg\",\"datePublished\":\"2024-08-06T17:06:42+00:00\",\"dateModified\":\"2025-07-07T15:18:03+00:00\",\"description\":\"Discover HAYNES\u00aeC-276 alloy, a nickel-chromium-molybdenum superalloy renowned for its outstanding resistance to pitting, crevice corrosion, and stress corrosion cracking in both oxidizing and reducing environments. Ideal for critical chemical processing, pollution control, and harsh industrial applications.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-c-276\\\/#breadcrumb\"},\"inLanguage\":\"en-US\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-c-276\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"en-US\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-c-276\\\/#primaryimage\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/c-276-alloy-hydrobromic-acid.jpg\",\"contentUrl\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/c-276-alloy-hydrobromic-acid.jpg\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-c-276\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Alloy Portfolio\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/\"},{\"@type\":\"ListItem\",\"position\":3,\"name\":\"Corrosion-resistant Alloys\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/\"},{\"@type\":\"ListItem\",\"position\":4,\"name\":\"HASTELLOY\u00ae C-276\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#website\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\",\"name\":\"Haynes International\",\"description\":\"The Home of HASTELLOY\u00ae and HAYNES\u00ae high-performance alloys\",\"publisher\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"en-US\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#organization\",\"name\":\"Haynes International\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"en-US\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/07\\\/logo.webp?fit=484%2C188&ssl=1\",\"contentUrl\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/07\\\/logo.webp?fit=484%2C188&ssl=1\",\"width\":484,\"height\":188,\"caption\":\"Haynes International\"},\"image\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/HaynesInternationalInc\\\/\",\"https:\\\/\\\/x.com\\\/HaynesIntl\",\"https:\\\/\\\/www.instagram.com\\\/haynesinternational\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/company\\\/haynes-international\\\/\"]}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"HASTELLOY\u00ae C-276 - Haynes International","description":"Discover HAYNES\u00aeC-276 alloy, a nickel-chromium-molybdenum superalloy renowned for its outstanding resistance to pitting, crevice corrosion, and stress corrosion cracking in both oxidizing and reducing environments. Ideal for critical chemical processing, pollution control, and harsh industrial applications.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/","og_locale":"en_US","og_type":"article","og_title":"HASTELLOY\u00ae C-276","og_description":"Discover HAYNES\u00aeC-276 alloy, a nickel-chromium-molybdenum superalloy renowned for its outstanding resistance to pitting, crevice corrosion, and stress corrosion cracking in both oxidizing and reducing environments. Ideal for critical chemical processing, pollution control, and harsh industrial applications.","og_url":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/","og_site_name":"Haynes International","article_publisher":"https:\/\/www.facebook.com\/HaynesInternationalInc\/","article_modified_time":"2025-07-07T15:18:03+00:00","og_image":[{"url":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrobromic-acid.jpg","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_site":"@HaynesIntl","twitter_misc":{"Est. reading time":"11 minutes"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"WebPage","@id":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/","url":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/","name":"HASTELLOY\u00ae C-276 - Haynes International","isPartOf":{"@id":"https:\/\/haynesintl.com\/en\/#website"},"primaryImageOfPage":{"@id":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/#primaryimage"},"image":{"@id":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/#primaryimage"},"thumbnailUrl":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrobromic-acid.jpg","datePublished":"2024-08-06T17:06:42+00:00","dateModified":"2025-07-07T15:18:03+00:00","description":"Discover HAYNES\u00aeC-276 alloy, a nickel-chromium-molybdenum superalloy renowned for its outstanding resistance to pitting, crevice corrosion, and stress corrosion cracking in both oxidizing and reducing environments. Ideal for critical chemical processing, pollution control, and harsh industrial applications.","breadcrumb":{"@id":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/#breadcrumb"},"inLanguage":"en-US","potentialAction":[{"@type":"ReadAction","target":["https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/"]}]},{"@type":"ImageObject","inLanguage":"en-US","@id":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/#primaryimage","url":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrobromic-acid.jpg","contentUrl":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/c-276-alloy-hydrobromic-acid.jpg"},{"@type":"BreadcrumbList","@id":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-c-276\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/haynesintl.com\/en\/"},{"@type":"ListItem","position":2,"name":"Alloy Portfolio","item":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/"},{"@type":"ListItem","position":3,"name":"Corrosion-resistant Alloys","item":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/"},{"@type":"ListItem","position":4,"name":"HASTELLOY\u00ae C-276"}]},{"@type":"WebSite","@id":"https:\/\/haynesintl.com\/en\/#website","url":"https:\/\/haynesintl.com\/en\/","name":"Haynes International","description":"The Home of HASTELLOY\u00ae and HAYNES\u00ae high-performance alloys","publisher":{"@id":"https:\/\/haynesintl.com\/en\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/haynesintl.com\/en\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"en-US"},{"@type":"Organization","@id":"https:\/\/haynesintl.com\/en\/#organization","name":"Haynes International","url":"https:\/\/haynesintl.com\/en\/","logo":{"@type":"ImageObject","inLanguage":"en-US","@id":"https:\/\/haynesintl.com\/en\/#\/schema\/logo\/image\/","url":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/07\/logo.webp?fit=484%2C188&ssl=1","contentUrl":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/07\/logo.webp?fit=484%2C188&ssl=1","width":484,"height":188,"caption":"Haynes International"},"image":{"@id":"https:\/\/haynesintl.com\/en\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/HaynesInternationalInc\/","https:\/\/x.com\/HaynesIntl","https:\/\/www.instagram.com\/haynesinternational\/","https:\/\/www.linkedin.com\/company\/haynes-international\/"]}]}},"jetpack_sharing_enabled":true,"_links":{"self":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys\/1973","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys"}],"about":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/types\/alloys"}],"author":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/users\/2"}],"version-history":[{"count":11,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys\/1973\/revisions"}],"predecessor-version":[{"id":12003,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys\/1973\/revisions\/12003"}],"up":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys\/29"}],"wp:attachment":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/media?parent=1973"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}