{"id":1965,"date":"2024-08-06T17:06:42","date_gmt":"2024-08-06T17:06:42","guid":{"rendered":"https:\/\/haynesintl.com\/alloys\/hastelloy-b-3\/"},"modified":"2025-07-07T15:05:36","modified_gmt":"2025-07-07T15:05:36","slug":"hastelloy-b-3","status":"publish","type":"alloys","link":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/","title":{"rendered":"HASTELLOY<sup>\u00ae<\/sup> B-3<sup>\u00ae<\/sup>"},"content":{"rendered":"\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-principal-features\">Principal Features<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;B-3<sup>\u00ae<\/sup>&nbsp;alloy (UNS N10675) exhibits extremely high resistance to pure hydrochloric, hydrobromic, and sulfuric acids. Furthermore, it has greatly improved structural stability compared with previous B-type alloys, leading to fewer concerns during welding, fabrication, and service.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Like other nickel alloys (in the mill annealed condition), it is ductile, can be formed and welded, and resists stress corrosion cracking in chloride-bearing solutions. Also, it is able to withstand fluoride-bearing media and concentrated sulfuric acid, both of which result in damage to zirconium alloys.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;B-3<sup>\u00ae<\/sup>&nbsp;alloy is available in the form of plates, sheets, strips, billets, bars, wires, pipes, tubes, and coated electrodes. It is used in numerous chemical process industry (CPI) applications, especially in the construction of reaction vessels for pure, reducing acid service.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">*Please contact our\u00a0<a href=\"\/contact\" rel=\"noopener\">technical support team<\/a>\u00a0if you have technical questions about this alloy.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-nominal-composition\">Nominal Composition<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-51\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"2\"\n           data-rows=\"17\"\n           data-wpID=\"51\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        Weight %                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Nickel                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65 min.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Molybdenum                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        28.5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Chromium                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Iron                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Tungsten                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Manganese                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Cobalt                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Aluminum                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.5 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Titanium                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.2 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Silicon                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.1 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Carbon                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Niobium                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.2 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A14\"\n                    data-col-index=\"0\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Vanadium                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.2 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A15\"\n                    data-col-index=\"0\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Copper                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.2 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Tantalum                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.2 max.                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A17\"\n                    data-col-index=\"0\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Zirconium                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01 max.                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-51'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-thermal-stability-t-t-t-chart\">Thermal Stability T T T Chart<\/h2>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"326\" height=\"350\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloy-b-3-time-temp-transformation.tmb-ze-350-350.jpg?resize=326%2C350&#038;ssl=1\" alt=\"\" class=\"wp-image-3008\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloy-b-3-time-temp-transformation.tmb-ze-350-350.jpg?w=326&amp;ssl=1 326w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloy-b-3-time-temp-transformation.tmb-ze-350-350.jpg?resize=279%2C300&amp;ssl=1 279w\" sizes=\"(max-width: 326px) 100vw, 326px\" \/><\/figure>\n<\/div>\n\n\n<p class=\"wp-block-paragraph\">The molybdenum content of the nickel-molybdenum (B-type) alloys is such that there is a strong tendency for phases other than the desirable (face-centered cubic) gamma phase to form in the microstructure, particularly in the temperature range 500\u00b0C to 900\u00b0C. The most deleterious of these alternate phases is Ni<sub>4<\/sub>Mo, which forms quickly at certain temperatures, affects ductility, and reduces resistance to stress corrosion cracking.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The chief attribute of B-3 alloy, as compared with other modern B-type materials, is its greatly improved structural stability (in particular its reduced susceptibility to Ni<sub>4<\/sub>Mo).<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The time-temperature-transformation diagram shown above illustrates the advantages of B-3 alloy over its predecessor (B-2 alloy). Whereas B-2 alloy suffers from the rapid formation of Ni<sub>4<\/sub>Mo at around 750\u00b0C, it takes several hours (at around 650\u00b0C), to induce deleterious second phases in B-3 alloy. This is due to the judicious use of minor elements and a shift in the molybdenum content, to induce the slowly-forming Ni<sub>3<\/sub>Mo instead.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-iso-corrosion-diagrams\">Iso Corrosion Diagrams<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Each of these iso-corrosion diagrams was constructed using numerous corrosion rate values, generated at different acid concentrations and temperatures (up to the boiling point). The blue line represents those combinations of acid concentration and temperature at which a corrosion rate of 0.1 mm\/y (4 mils per year) is expected, based on laboratory tests in reagent grade acids. Below the line, rates under 0.1 mm\/y are expected. The red line in the sulfuric acid diagram indicates the combinations of acid concentration and temperature at which a corrosion rate of 0.5 mm\/y (20 mils per year) is expected. Above the red line, rates over 0.5 mm\/y are expected. Between the blue and red lines, corrosion rates are expected to fall between 0.1 and 0.5 mm\/y. These diagrams do not predict the corrosion rates above the boiling point curves.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"349\" height=\"375\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-corrosion-in-hydrobromic-acid.jpg?resize=349%2C375&#038;ssl=1\" alt=\"\" class=\"wp-image-3012\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-corrosion-in-hydrobromic-acid.jpg?w=349&amp;ssl=1 349w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-corrosion-in-hydrobromic-acid.jpg?resize=279%2C300&amp;ssl=1 279w\" sizes=\"(max-width: 349px) 100vw, 349px\" \/><\/figure>\n<\/div>\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"349\" height=\"376\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-corrosion-in-hydrochloric-acid.jpg?resize=349%2C376&#038;ssl=1\" alt=\"\" class=\"wp-image-3016\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-corrosion-in-hydrochloric-acid.jpg?w=349&amp;ssl=1 349w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-corrosion-in-hydrochloric-acid.jpg?resize=278%2C300&amp;ssl=1 278w\" sizes=\"(max-width: 349px) 100vw, 349px\" \/><\/figure>\n<\/div>\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"349\" height=\"375\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-corrosion-in-phosphoric-acid.jpg?resize=349%2C375&#038;ssl=1\" alt=\"\" class=\"wp-image-3020\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-corrosion-in-phosphoric-acid.jpg?w=349&amp;ssl=1 349w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-corrosion-in-phosphoric-acid.jpg?resize=279%2C300&amp;ssl=1 279w\" sizes=\"(max-width: 349px) 100vw, 349px\" \/><\/figure>\n<\/div>\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"348\" height=\"374\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-corrosion-in-sulphuric-acid.jpg?resize=348%2C374&#038;ssl=1\" alt=\"\" class=\"wp-image-3024\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-corrosion-in-sulphuric-acid.jpg?w=348&amp;ssl=1 348w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-corrosion-in-sulphuric-acid.jpg?resize=279%2C300&amp;ssl=1 279w\" sizes=\"(max-width: 348px) 100vw, 348px\" \/><\/figure>\n<\/div><\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-selected-corrosion-data\">Selected Corrosion Data<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-hydrobromic-acid\">Hydrobromic Acid<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-52\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"10\"\n           data-rows=\"11\"\n           data-wpID=\"52\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" style=\"height:58px;\">\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Conc.\nWt.%                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        50\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        75\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        125\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        150\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        175\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        225\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"J1\"\n                    data-col-index=\"9\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Boiling                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107\u00b0C                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.24                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.12                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.43                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-52'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">All corrosion rates are in millimeters per year (mm\/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.<br>Data are from Corrosion Laboratory Jobs 71-97, 26-99, and 49-99.<br>All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"465\" height=\"500\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hydrobromic-b-3.tmb-ze-500-500.jpg?resize=465%2C500&#038;ssl=1\" alt=\"\" class=\"wp-image-3028\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hydrobromic-b-3.tmb-ze-500-500.jpg?w=465&amp;ssl=1 465w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hydrobromic-b-3.tmb-ze-500-500.jpg?resize=279%2C300&amp;ssl=1 279w\" sizes=\"(max-width: 465px) 100vw, 465px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-hydrochloric-acid\">Hydrochloric Acid<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-61\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"10\"\n           data-rows=\"15\"\n           data-wpID=\"61\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Conc.\n\nWt.%                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        50\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        75\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        125\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        150\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        175\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        225\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"J1\"\n                    data-col-index=\"9\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Boiling                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107\u00b0C                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J12\"\n                    data-col-index=\"9\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.24                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I13\"\n                    data-col-index=\"8\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J13\"\n                    data-col-index=\"9\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A14\"\n                    data-col-index=\"0\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.23                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I14\"\n                    data-col-index=\"8\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J14\"\n                    data-col-index=\"9\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.21                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A15\"\n                    data-col-index=\"0\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I15\"\n                    data-col-index=\"8\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J15\"\n                    data-col-index=\"9\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-61'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">All corrosion rates are in millimeters per year (mm\/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.<br>Data are from Corrosion Laboratory Jobs 37-92, 30-94, and 42-95.<br>All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"465\" height=\"500\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hydrochloric-b-3.tmb-ze-500-500.jpg?resize=465%2C500&#038;ssl=1\" alt=\"\" class=\"wp-image-3032\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hydrochloric-b-3.tmb-ze-500-500.jpg?w=465&amp;ssl=1 465w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hydrochloric-b-3.tmb-ze-500-500.jpg?resize=279%2C300&amp;ssl=1 279w\" sizes=\"(max-width: 465px) 100vw, 465px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-phosphoric-acid\">Phosphoric Acid<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-63\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"10\"\n           data-rows=\"11\"\n           data-wpID=\"63\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Conc.\nWt.%                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        125\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        150\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        175\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        225\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        250\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        275\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"J1\"\n                    data-col-index=\"9\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Boiling                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        121\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        135\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        149\u00b0C                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.21                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        75                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        85                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-63'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">All corrosion rates are in millimeters per year (mm\/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.<br>Data are from Corrosion Laboratory Jobs 113-92, 31-94, and 47-97.<br>All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"465\" height=\"500\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/phosphoric-b-3.tmb-ze-500-500.jpg?resize=465%2C500&#038;ssl=1\" alt=\"\" class=\"wp-image-3036\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/phosphoric-b-3.tmb-ze-500-500.jpg?w=465&amp;ssl=1 465w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/phosphoric-b-3.tmb-ze-500-500.jpg?resize=279%2C300&amp;ssl=1 279w\" sizes=\"(max-width: 465px) 100vw, 465px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-sulfuric-acid\">Sulfuric Acid<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-65\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"13\"\n           data-rows=\"17\"\n           data-wpID=\"65\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        Conc.\nWt.%                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        75\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        125\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        150\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        175\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        225\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I1\"\n                    data-col-index=\"8\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        250\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"J1\"\n                    data-col-index=\"9\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        275\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"K1\"\n                    data-col-index=\"10\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"L1\"\n                    data-col-index=\"11\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        350\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"M1\"\n                    data-col-index=\"12\"\n                    data-row-index=\"0\"\n                    style=\" width:7.6923076923077%;                    padding:10px;\n                    \"\n                    >\n                                        Boiling                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        121\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"J2\"\n                    data-col-index=\"9\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        135\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"K2\"\n                    data-col-index=\"10\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        149\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"L2\"\n                    data-col-index=\"11\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        177\u00b0C                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K3\"\n                    data-col-index=\"10\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L3\"\n                    data-col-index=\"11\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M3\"\n                    data-col-index=\"12\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K4\"\n                    data-col-index=\"10\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L4\"\n                    data-col-index=\"11\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M4\"\n                    data-col-index=\"12\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K5\"\n                    data-col-index=\"10\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L5\"\n                    data-col-index=\"11\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M5\"\n                    data-col-index=\"12\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K6\"\n                    data-col-index=\"10\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L6\"\n                    data-col-index=\"11\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M6\"\n                    data-col-index=\"12\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K7\"\n                    data-col-index=\"10\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L7\"\n                    data-col-index=\"11\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M7\"\n                    data-col-index=\"12\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K8\"\n                    data-col-index=\"10\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L8\"\n                    data-col-index=\"11\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M8\"\n                    data-col-index=\"12\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K9\"\n                    data-col-index=\"10\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L9\"\n                    data-col-index=\"11\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M9\"\n                    data-col-index=\"12\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K10\"\n                    data-col-index=\"10\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L10\"\n                    data-col-index=\"11\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M10\"\n                    data-col-index=\"12\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K11\"\n                    data-col-index=\"10\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L11\"\n                    data-col-index=\"11\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M11\"\n                    data-col-index=\"12\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J12\"\n                    data-col-index=\"9\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K12\"\n                    data-col-index=\"10\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L12\"\n                    data-col-index=\"11\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M12\"\n                    data-col-index=\"12\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I13\"\n                    data-col-index=\"8\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J13\"\n                    data-col-index=\"9\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K13\"\n                    data-col-index=\"10\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L13\"\n                    data-col-index=\"11\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M13\"\n                    data-col-index=\"12\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A14\"\n                    data-col-index=\"0\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I14\"\n                    data-col-index=\"8\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J14\"\n                    data-col-index=\"9\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K14\"\n                    data-col-index=\"10\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L14\"\n                    data-col-index=\"11\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M14\"\n                    data-col-index=\"12\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A15\"\n                    data-col-index=\"0\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I15\"\n                    data-col-index=\"8\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J15\"\n                    data-col-index=\"9\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K15\"\n                    data-col-index=\"10\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L15\"\n                    data-col-index=\"11\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.44                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M15\"\n                    data-col-index=\"12\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.76                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        90                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I16\"\n                    data-col-index=\"8\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J16\"\n                    data-col-index=\"9\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K16\"\n                    data-col-index=\"10\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L16\"\n                    data-col-index=\"11\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.76                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M16\"\n                    data-col-index=\"12\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A17\"\n                    data-col-index=\"0\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        96                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H17\"\n                    data-col-index=\"7\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I17\"\n                    data-col-index=\"8\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J17\"\n                    data-col-index=\"9\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.22                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"K17\"\n                    data-col-index=\"10\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.35                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"L17\"\n                    data-col-index=\"11\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.59                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"M17\"\n                    data-col-index=\"12\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-65'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">All corrosion rates are in millimeters per year (mm\/y); to convert to mils (thousandths of an inch) per year, divide by 0.0254.<br>Data are from Corrosion Laboratory Jobs 37-92, 29-94, 47-94, 42-95, and 14-96.<br>All tests were performed in reagent grade acids under laboratory conditions; field tests are encouraged prior to industrial use.<\/p>\n\n\n<div class=\"wp-block-image\">\n<figure class=\"aligncenter size-full\"><img data-recalc-dims=\"1\" decoding=\"async\" width=\"451\" height=\"477\" src=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-diagram-sulfuric-acid.tmb-ze-500-500.png?resize=451%2C477&#038;ssl=1\" alt=\"\" class=\"wp-image-3040\" srcset=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-diagram-sulfuric-acid.tmb-ze-500-500.png?w=451&amp;ssl=1 451w, https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/08\/b-3-iso-diagram-sulfuric-acid.tmb-ze-500-500.png?resize=284%2C300&amp;ssl=1 284w\" sizes=\"(max-width: 451px) 100vw, 451px\" \/><\/figure>\n<\/div>\n\n\n<h3 class=\"wp-block-heading\" id=\"h-reagent-grade-solutions-mm-y\">Reagent Grade Solutions, mm\/y<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-67\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"8\"\n           data-rows=\"42\"\n           data-wpID=\"67\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:12.515644555695%;                    padding:10px;\n                    \"\n                    >\n                                        Chemical                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:12.390488110138%;                    padding:10px;\n                    \"\n                    >\n                                        Conc.                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:12.515644555695%;                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:12.515644555695%;                    padding:10px;\n                    \"\n                    >\n                                        125\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:12.515644555695%;                    padding:10px;\n                    \"\n                    >\n                                        150\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:12.515644555695%;                    padding:10px;\n                    \"\n                    >\n                                        175\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:12.515644555695%;                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:12.515644555695%;                    padding:10px;\n                    \"\n                    >\n                                        Boiling                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        38\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        52\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        66\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        79\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93\u00b0C                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"5\"                     data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Acetic Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        99                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"6\"                     data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Formic Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        89                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"6\"                     data-cell-id=\"A14\"\n                    data-col-index=\"0\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Hydrobromic Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.24                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.12                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.27                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H17\"\n                    data-col-index=\"7\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B18\"\n                    data-col-index=\"1\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F18\"\n                    data-col-index=\"5\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G18\"\n                    data-col-index=\"6\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H18\"\n                    data-col-index=\"7\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B19\"\n                    data-col-index=\"1\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C19\"\n                    data-col-index=\"2\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F19\"\n                    data-col-index=\"5\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G19\"\n                    data-col-index=\"6\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H19\"\n                    data-col-index=\"7\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.43                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"6\"                     data-cell-id=\"A20\"\n                    data-col-index=\"0\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Hydrochloric Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B20\"\n                    data-col-index=\"1\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F20\"\n                    data-col-index=\"5\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G20\"\n                    data-col-index=\"6\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H20\"\n                    data-col-index=\"7\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B21\"\n                    data-col-index=\"1\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C21\"\n                    data-col-index=\"2\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D21\"\n                    data-col-index=\"3\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.16                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E21\"\n                    data-col-index=\"4\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F21\"\n                    data-col-index=\"5\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G21\"\n                    data-col-index=\"6\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.26                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H21\"\n                    data-col-index=\"7\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B22\"\n                    data-col-index=\"1\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C22\"\n                    data-col-index=\"2\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D22\"\n                    data-col-index=\"3\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.19                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E22\"\n                    data-col-index=\"4\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.25                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F22\"\n                    data-col-index=\"5\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G22\"\n                    data-col-index=\"6\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H22\"\n                    data-col-index=\"7\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B23\"\n                    data-col-index=\"1\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C23\"\n                    data-col-index=\"2\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D23\"\n                    data-col-index=\"3\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E23\"\n                    data-col-index=\"4\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.24                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F23\"\n                    data-col-index=\"5\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G23\"\n                    data-col-index=\"6\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H23\"\n                    data-col-index=\"7\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B24\"\n                    data-col-index=\"1\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C24\"\n                    data-col-index=\"2\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D24\"\n                    data-col-index=\"3\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.18                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E24\"\n                    data-col-index=\"4\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.23                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F24\"\n                    data-col-index=\"5\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G24\"\n                    data-col-index=\"6\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.28                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H24\"\n                    data-col-index=\"7\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.21                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B25\"\n                    data-col-index=\"1\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C25\"\n                    data-col-index=\"2\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D25\"\n                    data-col-index=\"3\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E25\"\n                    data-col-index=\"4\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.21                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F25\"\n                    data-col-index=\"5\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G25\"\n                    data-col-index=\"6\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H25\"\n                    data-col-index=\"7\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"7\"                     data-cell-id=\"A26\"\n                    data-col-index=\"0\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Phosphoric Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B26\"\n                    data-col-index=\"1\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C26\"\n                    data-col-index=\"2\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D26\"\n                    data-col-index=\"3\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E26\"\n                    data-col-index=\"4\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F26\"\n                    data-col-index=\"5\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G26\"\n                    data-col-index=\"6\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H26\"\n                    data-col-index=\"7\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B27\"\n                    data-col-index=\"1\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C27\"\n                    data-col-index=\"2\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D27\"\n                    data-col-index=\"3\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E27\"\n                    data-col-index=\"4\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F27\"\n                    data-col-index=\"5\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G27\"\n                    data-col-index=\"6\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H27\"\n                    data-col-index=\"7\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.07                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B28\"\n                    data-col-index=\"1\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C28\"\n                    data-col-index=\"2\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D28\"\n                    data-col-index=\"3\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E28\"\n                    data-col-index=\"4\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F28\"\n                    data-col-index=\"5\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G28\"\n                    data-col-index=\"6\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H28\"\n                    data-col-index=\"7\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B29\"\n                    data-col-index=\"1\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C29\"\n                    data-col-index=\"2\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D29\"\n                    data-col-index=\"3\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E29\"\n                    data-col-index=\"4\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F29\"\n                    data-col-index=\"5\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G29\"\n                    data-col-index=\"6\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H29\"\n                    data-col-index=\"7\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.14                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B30\"\n                    data-col-index=\"1\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C30\"\n                    data-col-index=\"2\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D30\"\n                    data-col-index=\"3\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E30\"\n                    data-col-index=\"4\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F30\"\n                    data-col-index=\"5\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G30\"\n                    data-col-index=\"6\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H30\"\n                    data-col-index=\"7\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.21                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B31\"\n                    data-col-index=\"1\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C31\"\n                    data-col-index=\"2\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D31\"\n                    data-col-index=\"3\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E31\"\n                    data-col-index=\"4\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F31\"\n                    data-col-index=\"5\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G31\"\n                    data-col-index=\"6\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H31\"\n                    data-col-index=\"7\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B32\"\n                    data-col-index=\"1\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        85                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C32\"\n                    data-col-index=\"2\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D32\"\n                    data-col-index=\"3\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E32\"\n                    data-col-index=\"4\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F32\"\n                    data-col-index=\"5\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G32\"\n                    data-col-index=\"6\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H32\"\n                    data-col-index=\"7\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.10                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"10\"                     data-cell-id=\"A33\"\n                    data-col-index=\"0\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sulfuric Acid                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B33\"\n                    data-col-index=\"1\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C33\"\n                    data-col-index=\"2\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D33\"\n                    data-col-index=\"3\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E33\"\n                    data-col-index=\"4\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F33\"\n                    data-col-index=\"5\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G33\"\n                    data-col-index=\"6\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H33\"\n                    data-col-index=\"7\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B34\"\n                    data-col-index=\"1\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C34\"\n                    data-col-index=\"2\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D34\"\n                    data-col-index=\"3\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E34\"\n                    data-col-index=\"4\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.08                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F34\"\n                    data-col-index=\"5\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G34\"\n                    data-col-index=\"6\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.11                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H34\"\n                    data-col-index=\"7\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B35\"\n                    data-col-index=\"1\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C35\"\n                    data-col-index=\"2\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D35\"\n                    data-col-index=\"3\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E35\"\n                    data-col-index=\"4\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F35\"\n                    data-col-index=\"5\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G35\"\n                    data-col-index=\"6\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H35\"\n                    data-col-index=\"7\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B36\"\n                    data-col-index=\"1\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C36\"\n                    data-col-index=\"2\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D36\"\n                    data-col-index=\"3\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E36\"\n                    data-col-index=\"4\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F36\"\n                    data-col-index=\"5\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G36\"\n                    data-col-index=\"6\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.06                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H36\"\n                    data-col-index=\"7\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B37\"\n                    data-col-index=\"1\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C37\"\n                    data-col-index=\"2\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D37\"\n                    data-col-index=\"3\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E37\"\n                    data-col-index=\"4\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F37\"\n                    data-col-index=\"5\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G37\"\n                    data-col-index=\"6\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H37\"\n                    data-col-index=\"7\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B38\"\n                    data-col-index=\"1\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C38\"\n                    data-col-index=\"2\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D38\"\n                    data-col-index=\"3\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E38\"\n                    data-col-index=\"4\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F38\"\n                    data-col-index=\"5\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G38\"\n                    data-col-index=\"6\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H38\"\n                    data-col-index=\"7\"\n                    data-row-index=\"37\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.05                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B39\"\n                    data-col-index=\"1\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C39\"\n                    data-col-index=\"2\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D39\"\n                    data-col-index=\"3\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E39\"\n                    data-col-index=\"4\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F39\"\n                    data-col-index=\"5\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G39\"\n                    data-col-index=\"6\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H39\"\n                    data-col-index=\"7\"\n                    data-row-index=\"38\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B40\"\n                    data-col-index=\"1\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        80                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C40\"\n                    data-col-index=\"2\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D40\"\n                    data-col-index=\"3\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E40\"\n                    data-col-index=\"4\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F40\"\n                    data-col-index=\"5\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G40\"\n                    data-col-index=\"6\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H40\"\n                    data-col-index=\"7\"\n                    data-row-index=\"39\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.76                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B41\"\n                    data-col-index=\"1\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        90                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C41\"\n                    data-col-index=\"2\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D41\"\n                    data-col-index=\"3\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E41\"\n                    data-col-index=\"4\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F41\"\n                    data-col-index=\"5\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G41\"\n                    data-col-index=\"6\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H41\"\n                    data-col-index=\"7\"\n                    data-row-index=\"40\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B42\"\n                    data-col-index=\"1\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        96                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C42\"\n                    data-col-index=\"2\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D42\"\n                    data-col-index=\"3\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E42\"\n                    data-col-index=\"4\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F42\"\n                    data-col-index=\"5\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G42\"\n                    data-col-index=\"6\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H42\"\n                    data-col-index=\"7\"\n                    data-row-index=\"41\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-67'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-resistance-to-stress-corrosion-cracking\">Resistance to Stress Corrosion Cracking<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">One of the chief attributes of the nickel alloys is their resistance to chloride-induced stress corrosion cracking. A common solution for assessing the resistance of materials to this extremely destructive form of attack is boiling 45% magnesium chloride (ASTM Standard G 36), typically with stressed U-bend samples. As is evident from the following results, the three nickel alloys, B-3<sup>\u00ae<\/sup>, C-276 and 625, are much more resistant to this form of attack than the comparative, austenitic stainless steels. The tests were stopped after 1,008 hours (six weeks).<\/p>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-69\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"2\"\n           data-rows=\"6\"\n           data-wpID=\"69\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" style=\"height:69px;\">\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:39.365079365079%;                    padding:10px;\n                    \"\n                    >\n                                        Alloy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:60.634920634921%;                    padding:10px;\n                    \"\n                    >\n                                        Time to Cracking                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" style=\"height:65px;\">\n                                <td class=\"wpdt-cell wpdt-bc-FFFFFF wpdt-tc-000000 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316L                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2 h                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" style=\"height:53px;\">\n                                <td class=\"wpdt-cell wpdt-bc-FFFFFF wpdt-tc-000000 wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        254SMO                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        24 h                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" style=\"height:61px;\">\n                                <td class=\"wpdt-cell wpdt-bc-FFFFFF wpdt-tc-000000 wpdt-bold\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        625                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        No cracking in 1,008 h                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" style=\"height:61px;\">\n                                <td class=\"wpdt-cell wpdt-bc-FFFFFF wpdt-tc-000000 wpdt-bold\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        C-276                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        No cracking in 1,008 h                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" style=\"height:74px;\">\n                                <td class=\"wpdt-cell wpdt-bc-FFFFFF wpdt-tc-000000 wpdt-bold\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B-3<sup>\u00ae<\/sup>                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold\"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        No cracking in 1,008 h                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-69'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-FFFFFF { background-color: #FFFFFF !important;}\n.wpdt-tc-000000 { color: #000000 !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-corrosion-resistance-of-welds\">Corrosion Resistance of Welds<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">To assess the resistance of welds to corrosion, Haynes International has chosen to test all-weld-metal samples, taken from the quadrants of cruciform assemblies, created using multiple gas metal arc (MIG) weld passes. Predictably, the inhomogeneous nature of weld microstructures leads to higher corrosion rates (than with homogeneous, wrought products) in some environments. Nevertheless, HASTELLOY B-3 alloy exhibits very high resistance to the key, inorganic acids, even in welded form, as shown in the following table:<\/p>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-72\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"9\"\n           data-rows=\"9\"\n           data-wpID=\"72\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" style=\"height:40px;\">\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:10.245901639344%;                    padding:10px;\n                    \"\n                    >\n                                        Chemical                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"2\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:25.819672131148%;                    padding:10px;\n                    \"\n                    >\n                                        Concentration                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"2\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:20.491803278689%;                    padding:10px;\n                    \"\n                    >\n                                        Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:49.180327868852%;                    padding:10px;\n                    \"\n                    >\n                                        Corrosion Rate                    <\/td>\n                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" style=\"height:32px;\">\n                                                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Weld Metal                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Wrought Base Metal                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        wt.%                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mpy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm\/y                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mpy                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm\/y                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        H<sub>2<\/sub>SO<sub>4<\/sub>                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.5                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.09                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        H<sub>2<\/sub>SO<sub>4<\/sub>                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.13                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.6                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        H<sub>2<\/sub>SO<sub>4<\/sub>                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.03                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.01                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        H<sub>2<\/sub>SO<sub>4<\/sub>                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        90                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.02                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HCl                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.8                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.3                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HCl                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.4                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.29                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-72'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEEF1 { background-color: #EEEEF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n<\/style>\n<\/div>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-physical-properties\">Physical Properties<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-73\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"5\"\n           data-rows=\"37\"\n           data-wpID=\"73\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:26.605504587156%;                    padding:10px;\n                    \"\n                    >\n                                        Physical Property                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:36.697247706422%;                    padding:10px;\n                    \"\n                    >\n                                        Customary Units                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:36.697247706422%;                    padding:10px;\n                    \"\n                    >\n                                        Metric Units                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Density                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">0.333 lb\/in<sup>3<\/sup><\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">9.22 g\/cm<sup>3<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"7\"                     data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Electrical Resistivity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        53.8 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.37 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        53.9 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.37 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54.1 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.37 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54.3 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.38 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54.4 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.38 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55.4 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.40 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        57.5 \u00b5ohm.in                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.43 \u00b5ohm.m                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"7\"                     data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Thermal Conductivity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">78 Btu.in\/h.ft<sup>2<\/sup>&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.2 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">83 Btu.in\/h.ft<sup>2<\/sup>&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        12.1 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">93 Btu.in\/h.ft<sup>2<\/sup>&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        13.4 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">104 Btu.in\/h.ft<sup>2<\/sup>&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        14.8 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">116 Btu.in\/h.ft<sup>2<\/sup>&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        16.3 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">129 Btu.in\/h.ft<sup>2<\/sup>&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17.9 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">142 Btu.in\/h.ft<sup>2<\/sup>&deg;F<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        19.6 W\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"6\"                     data-cell-id=\"A17\"\n                    data-col-index=\"0\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Mean Coefficient of\nThermal Expansion                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77-200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        5.7 \u00b5in\/in.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25-100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10.6 \u00b5m\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B18\"\n                    data-col-index=\"1\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77-400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C18\"\n                    data-col-index=\"2\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.1 \u00b5in\/in.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D18\"\n                    data-col-index=\"3\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25-200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E18\"\n                    data-col-index=\"4\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.1 \u00b5m\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B19\"\n                    data-col-index=\"1\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77-600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C19\"\n                    data-col-index=\"2\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.3 \u00b5in\/in.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D19\"\n                    data-col-index=\"3\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25-300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E19\"\n                    data-col-index=\"4\"\n                    data-row-index=\"18\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.4 \u00b5m\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B20\"\n                    data-col-index=\"1\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77-800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C20\"\n                    data-col-index=\"2\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.5 \u00b5in\/in.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D20\"\n                    data-col-index=\"3\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25-400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E20\"\n                    data-col-index=\"4\"\n                    data-row-index=\"19\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.6 \u00b5m\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B21\"\n                    data-col-index=\"1\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77-1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C21\"\n                    data-col-index=\"2\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.6 \u00b5in\/in.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D21\"\n                    data-col-index=\"3\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25-500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E21\"\n                    data-col-index=\"4\"\n                    data-row-index=\"20\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.8 \u00b5m\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B22\"\n                    data-col-index=\"1\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        77-1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C22\"\n                    data-col-index=\"2\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        6.5 \u00b5in\/in.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D22\"\n                    data-col-index=\"3\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        25-600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E22\"\n                    data-col-index=\"4\"\n                    data-row-index=\"21\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        11.8 \u00b5m\/m.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"7\"                     data-cell-id=\"A23\"\n                    data-col-index=\"0\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Specific Heat                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B23\"\n                    data-col-index=\"1\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C23\"\n                    data-col-index=\"2\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.089 Btu\/lb.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D23\"\n                    data-col-index=\"3\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E23\"\n                    data-col-index=\"4\"\n                    data-row-index=\"22\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        373 J\/kg.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B24\"\n                    data-col-index=\"1\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C24\"\n                    data-col-index=\"2\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.092 Btu\/lb.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D24\"\n                    data-col-index=\"3\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E24\"\n                    data-col-index=\"4\"\n                    data-row-index=\"23\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        382 J\/kg.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B25\"\n                    data-col-index=\"1\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C25\"\n                    data-col-index=\"2\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.098 Btu\/lb.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D25\"\n                    data-col-index=\"3\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E25\"\n                    data-col-index=\"4\"\n                    data-row-index=\"24\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        409 J\/kg.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B26\"\n                    data-col-index=\"1\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C26\"\n                    data-col-index=\"2\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.102 Btu\/lb.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D26\"\n                    data-col-index=\"3\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E26\"\n                    data-col-index=\"4\"\n                    data-row-index=\"25\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        421 J\/kg.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B27\"\n                    data-col-index=\"1\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C27\"\n                    data-col-index=\"2\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.104 Btu\/lb.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D27\"\n                    data-col-index=\"3\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E27\"\n                    data-col-index=\"4\"\n                    data-row-index=\"26\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        431 J\/kg.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B28\"\n                    data-col-index=\"1\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C28\"\n                    data-col-index=\"2\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.104 Btu\/lb.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D28\"\n                    data-col-index=\"3\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E28\"\n                    data-col-index=\"4\"\n                    data-row-index=\"27\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        436 J\/kg.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B29\"\n                    data-col-index=\"1\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C29\"\n                    data-col-index=\"2\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.112 Btu\/lb.\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D29\"\n                    data-col-index=\"3\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E29\"\n                    data-col-index=\"4\"\n                    data-row-index=\"28\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        434 J\/kg.\u00b0C                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"7\"                     data-cell-id=\"A30\"\n                    data-col-index=\"0\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Dynamic Modulus\nof Elasticity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B30\"\n                    data-col-index=\"1\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C30\"\n                    data-col-index=\"2\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">31.4 x 10<sup>6<\/sup>psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D30\"\n                    data-col-index=\"3\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E30\"\n                    data-col-index=\"4\"\n                    data-row-index=\"29\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        216 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B31\"\n                    data-col-index=\"1\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C31\"\n                    data-col-index=\"2\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">30.9 x 10<sup>6<\/sup>psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D31\"\n                    data-col-index=\"3\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        100\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E31\"\n                    data-col-index=\"4\"\n                    data-row-index=\"30\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        213 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B32\"\n                    data-col-index=\"1\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C32\"\n                    data-col-index=\"2\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">30.1 x 10<sup>6<\/sup>psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D32\"\n                    data-col-index=\"3\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E32\"\n                    data-col-index=\"4\"\n                    data-row-index=\"31\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        208 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B33\"\n                    data-col-index=\"1\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C33\"\n                    data-col-index=\"2\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">29.3 x 10<sup>6<\/sup>psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D33\"\n                    data-col-index=\"3\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        300\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E33\"\n                    data-col-index=\"4\"\n                    data-row-index=\"32\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        202 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B34\"\n                    data-col-index=\"1\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C34\"\n                    data-col-index=\"2\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">28.3 x 10<sup>6<\/sup>psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D34\"\n                    data-col-index=\"3\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E34\"\n                    data-col-index=\"4\"\n                    data-row-index=\"33\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        197 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B35\"\n                    data-col-index=\"1\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C35\"\n                    data-col-index=\"2\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">27.2 x 10<sup>6<\/sup>psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D35\"\n                    data-col-index=\"3\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        500\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E35\"\n                    data-col-index=\"4\"\n                    data-row-index=\"34\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        190 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B36\"\n                    data-col-index=\"1\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C36\"\n                    data-col-index=\"2\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">26.5 x 10<sup>6<\/sup>psi<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D36\"\n                    data-col-index=\"3\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E36\"\n                    data-col-index=\"4\"\n                    data-row-index=\"35\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        185 GPa                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A37\"\n                    data-col-index=\"0\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Melting Range                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B37\"\n                    data-col-index=\"1\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2500-2585\u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C37\"\n                    data-col-index=\"2\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D37\"\n                    data-col-index=\"3\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1370-1418\u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E37\"\n                    data-col-index=\"4\"\n                    data-row-index=\"36\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-73'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*RT= Room Temperature<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-impact-strength\">Impact Strength<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-75\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"8\"\n           data-rows=\"10\"\n           data-wpID=\"75\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" style=\"height:6px;\">\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:11.9189511323%;                    padding:10px;\n                    \"\n                    >\n                                        Form                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:23.837902264601%;                    padding:10px;\n                    \"\n                    >\n                                        Thickness\/Diameter                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:23.837902264601%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:23.837902264601%;                    padding:10px;\n                    \"\n                    >\n                                        Impact Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:16.567342073897%;                    padding:10px;\n                    \"\n                    >\n                                        Numberof Tests                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" style=\"height:35px;\">\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ft.lbf                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        J                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.79                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        353                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        479                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.79                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -320                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -196                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        334                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        453                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.38                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        35                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        388                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        526                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.38                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        35                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -320                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -196                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        359                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        487                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Bar                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.58                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        388                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        526                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Bar                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.58                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -320                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -196                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        339                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        460                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Bar                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.97                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        390                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        529                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Bar                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1.97                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -320                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -196                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        338                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        458                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-75'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Charpy V-Notch Samples.<br>RT= Room Temperature<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-tensile-strength-and-elongation\">Tensile Strength and Elongation<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-77\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"10\"\n           data-rows=\"16\"\n           data-wpID=\"77\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Form                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Thickness                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Test Temperature                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        0.2% Yield Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"H1\"\n                    data-col-index=\"7\"\n                    data-row-index=\"0\"\n                    style=\" width:20%;                    padding:10px;\n                    \"\n                    >\n                                        Ultimate Tensile Strength                    <\/td>\n                                                            <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold\"\n                                            data-cell-id=\"J1\"\n                    data-col-index=\"9\"\n                    data-row-index=\"0\"\n                    style=\" width:10%;                    padding:10px;\n                    \"\n                    >\n                                        Elongation                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        mm                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0F                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u00b0C                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"H2\"\n                    data-col-index=\"7\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ksi                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"I2\"\n                    data-col-index=\"8\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        MPa                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEEF1 wpdt-tc-444444 wpdt-bold\"\n                                            data-cell-id=\"J2\"\n                    data-col-index=\"9\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        %                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.125                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        421                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H3\"\n                    data-col-index=\"7\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        125                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I3\"\n                    data-col-index=\"8\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        862                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J3\"\n                    data-col-index=\"9\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        53                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.125                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        55                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        379                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H4\"\n                    data-col-index=\"7\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        121                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I4\"\n                    data-col-index=\"8\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        834                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J4\"\n                    data-col-index=\"9\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        57                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.125                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        204                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        47                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        324                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H5\"\n                    data-col-index=\"7\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        110                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I5\"\n                    data-col-index=\"8\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        758                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J5\"\n                    data-col-index=\"9\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        60                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.125                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        303                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H6\"\n                    data-col-index=\"7\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        104                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I6\"\n                    data-col-index=\"8\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        717                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J6\"\n                    data-col-index=\"9\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        63                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.125                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        427                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        42                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        290                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H7\"\n                    data-col-index=\"7\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        102                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I7\"\n                    data-col-index=\"8\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        703                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J7\"\n                    data-col-index=\"9\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.125                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        39                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        269                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H8\"\n                    data-col-index=\"7\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        98                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I8\"\n                    data-col-index=\"8\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        676                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J8\"\n                    data-col-index=\"9\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        59                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.125                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        46                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        317                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H9\"\n                    data-col-index=\"7\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        104                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I9\"\n                    data-col-index=\"8\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        717                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J9\"\n                    data-col-index=\"9\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        56                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Multiple*                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        RT                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        58                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H10\"\n                    data-col-index=\"7\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        128                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I10\"\n                    data-col-index=\"8\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        883                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J10\"\n                    data-col-index=\"9\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        58                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Multiple*                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        54                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        372                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H11\"\n                    data-col-index=\"7\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        122                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I11\"\n                    data-col-index=\"8\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        841                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J11\"\n                    data-col-index=\"9\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        58                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Multiple*                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        400                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        204                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        48                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        331                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H12\"\n                    data-col-index=\"7\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        115                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I12\"\n                    data-col-index=\"8\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        793                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J12\"\n                    data-col-index=\"9\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        61                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Multiple*                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        600                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        316                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        44                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        303                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H13\"\n                    data-col-index=\"7\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        111                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I13\"\n                    data-col-index=\"8\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        765                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J13\"\n                    data-col-index=\"9\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A14\"\n                    data-col-index=\"0\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Multiple*                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        427                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        41                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        283                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H14\"\n                    data-col-index=\"7\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        108                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I14\"\n                    data-col-index=\"8\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        745                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J14\"\n                    data-col-index=\"9\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A15\"\n                    data-col-index=\"0\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Multiple*                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1000                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        538                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        276                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H15\"\n                    data-col-index=\"7\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        106                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I15\"\n                    data-col-index=\"8\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        731                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J15\"\n                    data-col-index=\"9\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        62                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Multiple*                    <\/td>\n                                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        1200                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        649                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        42                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        290                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"H16\"\n                    data-col-index=\"7\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        107                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"I16\"\n                    data-col-index=\"8\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        738                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"J16\"\n                    data-col-index=\"9\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        65                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-77'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEEF1 { background-color: #EEEEF1 !important;}\n.wpdt-tc-444444 { color: #444444 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">*Average values from the testing of 6 lots of plate (of different thicknesses) from three heats.<br>RT= Room Temperature<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-hardness\">Hardness<\/h2>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-78\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"3\"\n           data-rows=\"4\"\n           data-wpID=\"78\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:25%;                    padding:10px;\n                    \"\n                    >\n                                        Form                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:39.356435643564%;                    padding:10px;\n                    \"\n                    >\n                                        Hardness, HRBW                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:35.643564356436%;                    padding:10px;\n                    \"\n                    >\n                                        Typical ASTM Grain Size                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        93                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        4.5 \u2013 6.5                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Plate                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        95                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        3.5 \u2013 7                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Bar                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        92                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        2 \u2013 7.5                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-78'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">All samples tested in solution-annealed condition.<br>HRBW = Hardness Rockwell \u201cB\u201d, Tungsten Indentor.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-welding-and-fabrication\">Welding and Fabrication<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;B-3<sup>\u00ae<\/sup>&nbsp;alloy is very amenable to the Gas Metal Arc (GMA\/MIG), Gas Tungsten Arc (GTA\/TIG), and Shielded Metal Arc (SMA\/Stick) welding processes. For matching filler metals (i.e. solid wires and coated electrodes) that are available for these processes, and welding guidelines, please&nbsp;<a href=\"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/Fabrication-and-Welding-Brochure.pdf\" target=\"_blank\" rel=\"noreferrer noopener\">click here<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Wrought products of HASTELLOY<sup>\u00ae<\/sup>&nbsp;B-3<sup>\u00ae<\/sup>&nbsp;alloy are supplied in the Mill Annealed (MA) condition, unless otherwise specified. This solution annealing procedure has been developed to optimize the alloy\u2019s corrosion resistance and ductility. Following all hot forming operations, the material should be re-annealed, to restore optimum properties. In the case of cold-formed components of B-3<sup>\u00ae<\/sup>&nbsp;alloy, solution annealing should be performed prior to subsequent fabrication\/welding when cold work is greater than about 7%. Otherwise, B-3<sup>\u00ae<\/sup>&nbsp;alloy is very susceptible to cracking in the welded region during subsequent fabrication\/welding. The cracking may not become obvious until the component has been put into service. Care should also be taken to utilize well-controlled furnace annealing conditions: fast heat-up rate, precise temperature control, and rapid cooling.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The annealing temperature for HASTELLOY<sup>\u00ae<\/sup>&nbsp;B-3<sup>\u00ae<\/sup>&nbsp;alloy is 1066\u00b0C (1950\u00b0F), and water quenching is advised (rapid air cooling is feasible with structures thinner than 10 mm (0.375 in). A hold time at the annealing temperature of 10 to 30 minutes is recommended, depending on the thickness of the structure (thicker structures need the full 30 minutes). &nbsp;For more details concerning the heat treatment of HASTELLOY<sup>\u00ae<\/sup>&nbsp;B-3<sup>\u00ae<\/sup>&nbsp;alloy, please&nbsp;<a href=\"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/Fabrication-and-Welding-Brochure.pdf\" target=\"_blank\" rel=\"noreferrer noopener\">click here<\/a><a href=\"https:\/\/haynesintl.com\/alloys\/fabrication-brochure\/heat-treatment\" target=\"_blank\" rel=\"noopener\">.<\/a><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">HASTELLOY<sup>\u00ae<\/sup>&nbsp;B-3<sup>\u00ae<\/sup>&nbsp;alloy can be hot forged, hot rolled, hot upset, hot extruded, and hot formed. However, it is more sensitive to strain and strain rates than the austenitic stainless steels, and the hot working temperature range is quite narrow. For example, the recommended start temperature for hot forging is 1232\u00b0C (2250\u00b0F) and the recommended finish temperature is 982\u00b0C (1800\u00b0F).<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Moderate reductions and frequent re-heating provide the best results, as described&nbsp;<a href=\"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/Fabrication-and-Welding-Brochure.pdf\" target=\"_blank\" rel=\"noreferrer noopener\">here<\/a>.&nbsp;This reference also provides guidelines for cold forming, spinning, drop hammering, punching, and shearing. The alloy is stiffer than most austenitic stainless steels, and more energy is required during cold forming. Also, HASTELLOY<sup>\u00ae<\/sup>&nbsp;B-3<sup>\u00ae<\/sup>&nbsp;alloy work hardens more readily than most austenitic stainless steels, and may require several stages of cold work, with intermediate anneals.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">While cold work does not usually affect the resistance of HASTELLOY<sup>\u00ae<\/sup>&nbsp;B-3<sup>\u00ae<\/sup>&nbsp;alloy to general corrosion, it can affect resistance to stress corrosion cracking. For optimum corrosion performance, therefore, the re-annealing of cold worked parts (following an outer fiber elongation of 7% or more) is important. Cold or hot formed heads should always be annealed after forming, regardless of forming strain level. This is especially important if the material is to be subsequently welded.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-specifications-and-codes\">Specifications and Codes<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-specifications\">Specifications<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-79\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"2\"\n           data-rows=\"12\"\n           data-wpID=\"79\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        HASTELLOY<sup>\u00ae<\/sup> B-3<sup>\u00ae<\/sup> alloy\n(N10675, W80675)                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Sheet, Plate & Strip                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 333\/B 333 \nP= 44                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Billet, Rod & Bar                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 335\/B 335 \nB 472 \nP= 44                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Coated Electrodes                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SFA 5.11\/\u00a0A5.11 (ENiMo-10) F= 44                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Bare Welding Rods & Wire                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SFA 5.14\/\u00a0A5.14 (ERNiMo-10) F= 44                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Seamless Pipe & Tube                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 622\/B 622 P= 44                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Welded Pipe & Tube                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 619\/B 619 P= 44                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A8\"\n                    data-col-index=\"0\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Fittings                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 366\/B 366 P= 44                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A9\"\n                    data-col-index=\"0\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Forgings                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        SB 564\/B 564 P= 44                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        DIN                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        17744 No. 2.4600 NiMo29Cr                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A11\"\n                    data-col-index=\"0\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        T\u00dcV                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Werkstoffblatt 517 Kennblatt 7615.00 Kennblatt 7616.00 Kennblatt 7617.00                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Others                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        \u2013                    <\/td>\n                                        <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-79'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\" id=\"h-codes\">Codes<\/h3>\n\n\n\n<div class=\"wp-block-wpdatatables-wpdatatables-gutenberg-block\">\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-646\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"4\"\n           data-rows=\"13\"\n           data-wpID=\"646\"\n           data-responsive=\"0\"\n           data-has-header=\"0\">\n\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-063D71 wpdt-tc-FFFFFF wpdt-bold wpdt-merged-cell \"\n                     colspan=\"4\"  rowspan=\"1\"                     data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:100%;                    padding:10px;\n                    \"\n                    >\n                                        HASTELLOY<sup>\u00ae<\/sup> B-3<sup>\u00ae<\/sup> alloy\n(N10675, W80675)                    <\/td>\n                                                                            <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"11\"                     data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        ASME                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section l                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section lll                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Class 1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Class 2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Class 3                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800&ordm;F (427&ordm;C)<sup>1<\/sup>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section Vlll                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Div. 1                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800&ordm;F (427&ordm;C)<sup>1<\/sup>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                                        <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Div. 2                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Section Xll                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        650&deg;F (343&deg;C)<sup>2<\/sup>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B16.5                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800&deg;F (427&deg;C)<sup>3<\/sup>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B16.34                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800&deg;F (427&deg;C)<sup>4<\/sup>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B31.1                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold\"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        B31.3                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        800&deg;F (427&deg;C)<sup>5<\/sup>                    <\/td>\n                                                    <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1 wpdt-bold wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"A13\"\n                    data-col-index=\"0\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        VdT\u00dcV (doc #)                    <\/td>\n                                                            <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"2\"  rowspan=\"1\"                     data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        752&deg;F (400&ordm;C)<sup>6<\/sup>\n#517                    <\/td>\n                                                    <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-646'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\"><sup>1<\/sup>Plate, Sheet, Bar, Forgings, welded pipe\/tube, seamless pipe\/tube<br><sup>2<\/sup>Plate, Sheet, Bar, Forgings, fittings, welded pipe\/tube&nbsp;<sup>3<\/sup>Plate, Forgings, fittings<br><sup>4<\/sup>Plate, Bar, Forgings, seamless pipe\/tube<br><sup>5<\/sup>Plate, Sheet, Bar, fittings, welded pipe\/tube, seamless pipe\/tube<br><sup>6<\/sup>Plate, Shzeet, Bar, Forgings<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-disclaimer\">Disclaimer<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Haynes International makes all reasonable efforts to ensure the accuracy and correctness of the data displayed on this site but makes no representations or warranties as to the data\u2019s accuracy, correctness or reliability. All data are for general information only and not for providing design advice. Alloy properties disclosed here are based on work conducted principally by Haynes International, Inc. and occasionally supplemented by information from the open literature and, as such, are indicative only of the results of such tests and should not be considered guaranteed maximums or minimums.&nbsp; It is the responsibility of the user to test specific alloys under actual service conditions to determine their suitability for a particular purpose.For specific concentrations of elements present in a particular product and a discussion of the potential health affects thereof, refer to the Safety Data Sheets supplied by Haynes International, Inc.&nbsp; All trademarks are owned by Haynes International, Inc., unless otherwise indicated.<\/p>\n<\/div><\/div>\n\n\n\n<div class=\"wp-block-group\"><div class=\"wp-block-group__inner-container is-layout-constrained wp-block-group-is-layout-constrained\">\n<h2 class=\"wp-block-heading\" id=\"h-alloy-brochure\">Alloy Brochure<\/h2>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/pdf-alloy-b-3.pdf\">Download<\/a><\/div>\n<\/div>\n<\/div><\/div>\n","protected":false},"excerpt":{"rendered":"<p>Principal Features HASTELLOY<sup>\u00ae<\/sup>&nbsp;B-3<sup>\u00ae<\/sup>&nbsp;alloy (UNS N10675) exhibits extremely high resistance to pure hydrochloric, hydrobromic, and sulfuric acids. Furthermore, it has greatly improved structural stability compared with previous B-type alloys, leading to fewer concerns during welding, fabrication, and service. Like other nickel alloys (in the mill annealed condition), it is ductile, can be formed and welded, and [\u2026]<\/p>\n","protected":false},"author":2,"featured_media":0,"parent":29,"menu_order":0,"template":"","meta":{"_acf_changed":false,"_searchwp_excluded":"","inline_featured_image":false,"footnotes":""},"class_list":["post-1965","alloys","type-alloys","status-publish","hentry"],"acf":[],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v27.8 (Yoast SEO v28.4) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>HASTELLOY\u00ae B-3\u00ae - Haynes International<\/title>\n<meta name=\"description\" content=\"Discover HAYNES\u00aeB-3\u00ae alloy, a nickel-molybdenum superalloy offering exceptional resistance to hydrochloric, sulfuric, phosphoric, and other non-oxidizing acids. Engineered for enhanced thermal and structural stability compared to B-2, it resists stress-corrosion cracking and high-temperature embrittlement which is ideal for chemical process vessels, reactors, and acid-handling applications.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/\" \/>\n<meta property=\"og:locale\" content=\"en_US\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"HASTELLOY\u00ae B-3\u00ae\" \/>\n<meta property=\"og:description\" content=\"Discover HAYNES\u00aeB-3\u00ae alloy, a nickel-molybdenum superalloy offering exceptional resistance to hydrochloric, sulfuric, phosphoric, and other non-oxidizing acids. Engineered for enhanced thermal and structural stability compared to B-2, it resists stress-corrosion cracking and high-temperature embrittlement which is ideal for chemical process vessels, reactors, and acid-handling applications.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/\" \/>\n<meta property=\"og:site_name\" content=\"Haynes International\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/HaynesInternationalInc\/\" \/>\n<meta property=\"article:modified_time\" content=\"2025-07-07T15:05:36+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloy-b-3-time-temp-transformation.tmb-ze-350-350.jpg\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:site\" content=\"@HaynesIntl\" \/>\n<meta name=\"twitter:label1\" content=\"Est. reading time\" \/>\n\t<meta name=\"twitter:data1\" content=\"9 minutes\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-b-3\\\/\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-b-3\\\/\",\"name\":\"HASTELLOY\u00ae B-3\u00ae - Haynes International\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-b-3\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-b-3\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/hastelloy-b-3-time-temp-transformation.tmb-ze-350-350.jpg\",\"datePublished\":\"2024-08-06T17:06:42+00:00\",\"dateModified\":\"2025-07-07T15:05:36+00:00\",\"description\":\"Discover HAYNES\u00aeB-3\u00ae alloy, a nickel-molybdenum superalloy offering exceptional resistance to hydrochloric, sulfuric, phosphoric, and other non-oxidizing acids. Engineered for enhanced thermal and structural stability compared to B-2, it resists stress-corrosion cracking and high-temperature embrittlement which is ideal for chemical process vessels, reactors, and acid-handling applications.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-b-3\\\/#breadcrumb\"},\"inLanguage\":\"en-US\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-b-3\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"en-US\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-b-3\\\/#primaryimage\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/hastelloy-b-3-time-temp-transformation.tmb-ze-350-350.jpg\",\"contentUrl\":\"https:\\\/\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/08\\\/hastelloy-b-3-time-temp-transformation.tmb-ze-350-350.jpg\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/hastelloy-b-3\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Alloy Portfolio\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/\"},{\"@type\":\"ListItem\",\"position\":3,\"name\":\"Corrosion-resistant Alloys\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/alloy-portfolio\\\/corrosion-resistant-alloys\\\/\"},{\"@type\":\"ListItem\",\"position\":4,\"name\":\"HASTELLOY\u00ae B-3\u00ae\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#website\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\",\"name\":\"Haynes International\",\"description\":\"The Home of HASTELLOY\u00ae and HAYNES\u00ae high-performance alloys\",\"publisher\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"en-US\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#organization\",\"name\":\"Haynes International\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"en-US\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/07\\\/logo.webp?fit=484%2C188&ssl=1\",\"contentUrl\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/07\\\/logo.webp?fit=484%2C188&ssl=1\",\"width\":484,\"height\":188,\"caption\":\"Haynes International\"},\"image\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/HaynesInternationalInc\\\/\",\"https:\\\/\\\/x.com\\\/HaynesIntl\",\"https:\\\/\\\/www.instagram.com\\\/haynesinternational\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/company\\\/haynes-international\\\/\"]}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"HASTELLOY\u00ae B-3\u00ae - Haynes International","description":"Discover HAYNES\u00aeB-3\u00ae alloy, a nickel-molybdenum superalloy offering exceptional resistance to hydrochloric, sulfuric, phosphoric, and other non-oxidizing acids. Engineered for enhanced thermal and structural stability compared to B-2, it resists stress-corrosion cracking and high-temperature embrittlement which is ideal for chemical process vessels, reactors, and acid-handling applications.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/","og_locale":"en_US","og_type":"article","og_title":"HASTELLOY\u00ae B-3\u00ae","og_description":"Discover HAYNES\u00aeB-3\u00ae alloy, a nickel-molybdenum superalloy offering exceptional resistance to hydrochloric, sulfuric, phosphoric, and other non-oxidizing acids. Engineered for enhanced thermal and structural stability compared to B-2, it resists stress-corrosion cracking and high-temperature embrittlement which is ideal for chemical process vessels, reactors, and acid-handling applications.","og_url":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/","og_site_name":"Haynes International","article_publisher":"https:\/\/www.facebook.com\/HaynesInternationalInc\/","article_modified_time":"2025-07-07T15:05:36+00:00","og_image":[{"url":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloy-b-3-time-temp-transformation.tmb-ze-350-350.jpg","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_site":"@HaynesIntl","twitter_misc":{"Est. reading time":"9 minutes"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"WebPage","@id":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/","url":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/","name":"HASTELLOY\u00ae B-3\u00ae - Haynes International","isPartOf":{"@id":"https:\/\/haynesintl.com\/en\/#website"},"primaryImageOfPage":{"@id":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/#primaryimage"},"image":{"@id":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/#primaryimage"},"thumbnailUrl":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloy-b-3-time-temp-transformation.tmb-ze-350-350.jpg","datePublished":"2024-08-06T17:06:42+00:00","dateModified":"2025-07-07T15:05:36+00:00","description":"Discover HAYNES\u00aeB-3\u00ae alloy, a nickel-molybdenum superalloy offering exceptional resistance to hydrochloric, sulfuric, phosphoric, and other non-oxidizing acids. Engineered for enhanced thermal and structural stability compared to B-2, it resists stress-corrosion cracking and high-temperature embrittlement which is ideal for chemical process vessels, reactors, and acid-handling applications.","breadcrumb":{"@id":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/#breadcrumb"},"inLanguage":"en-US","potentialAction":[{"@type":"ReadAction","target":["https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/"]}]},{"@type":"ImageObject","inLanguage":"en-US","@id":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/#primaryimage","url":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloy-b-3-time-temp-transformation.tmb-ze-350-350.jpg","contentUrl":"https:\/\/haynesintl.com\/wp-content\/uploads\/2024\/08\/hastelloy-b-3-time-temp-transformation.tmb-ze-350-350.jpg"},{"@type":"BreadcrumbList","@id":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/hastelloy-b-3\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/haynesintl.com\/en\/"},{"@type":"ListItem","position":2,"name":"Alloy Portfolio","item":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/"},{"@type":"ListItem","position":3,"name":"Corrosion-resistant Alloys","item":"https:\/\/haynesintl.com\/en\/alloys\/alloy-portfolio\/corrosion-resistant-alloys\/"},{"@type":"ListItem","position":4,"name":"HASTELLOY\u00ae B-3\u00ae"}]},{"@type":"WebSite","@id":"https:\/\/haynesintl.com\/en\/#website","url":"https:\/\/haynesintl.com\/en\/","name":"Haynes International","description":"The Home of HASTELLOY\u00ae and HAYNES\u00ae high-performance alloys","publisher":{"@id":"https:\/\/haynesintl.com\/en\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/haynesintl.com\/en\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"en-US"},{"@type":"Organization","@id":"https:\/\/haynesintl.com\/en\/#organization","name":"Haynes International","url":"https:\/\/haynesintl.com\/en\/","logo":{"@type":"ImageObject","inLanguage":"en-US","@id":"https:\/\/haynesintl.com\/en\/#\/schema\/logo\/image\/","url":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/07\/logo.webp?fit=484%2C188&ssl=1","contentUrl":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/07\/logo.webp?fit=484%2C188&ssl=1","width":484,"height":188,"caption":"Haynes International"},"image":{"@id":"https:\/\/haynesintl.com\/en\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/HaynesInternationalInc\/","https:\/\/x.com\/HaynesIntl","https:\/\/www.instagram.com\/haynesinternational\/","https:\/\/www.linkedin.com\/company\/haynes-international\/"]}]}},"jetpack_sharing_enabled":true,"_links":{"self":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys\/1965","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys"}],"about":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/types\/alloys"}],"author":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/users\/2"}],"version-history":[{"count":7,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys\/1965\/revisions"}],"predecessor-version":[{"id":11994,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys\/1965\/revisions\/11994"}],"up":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys\/29"}],"wp:attachment":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/media?parent=1965"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}