{"id":108,"date":"2024-06-29T01:44:39","date_gmt":"2024-06-29T01:44:39","guid":{"rendered":"https:\/\/haynesintl.com\/alloys\/machining\/"},"modified":"2025-07-18T14:29:05","modified_gmt":"2025-07-18T14:29:05","slug":"machining","status":"publish","type":"alloys","link":"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/","title":{"rendered":"Machining"},"content":{"rendered":"\n<p class=\"wp-block-paragraph\"><strong>Recommended Tools and Machining Parameters Applicable to:<\/strong><br><strong>Corrosion-resistant Alloys<\/strong><strong><br>High-temperature Alloys<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Be aware that the cobalt-base alloys in these categories (25 and 188) can require different feeds and speeds (as noted in the table) than the nickel- and iron-based alloys.<\/em><\/p>\n\n\n\n<div class=\"wpdt-c row wpDataTableContainerSimpleTable wpDataTables wpDataTablesWrapper\n\"\n    >\n        <table id=\"wpdtSimpleTable-874\"\n           style=\"border-collapse:collapse;\n                   border-spacing:0px;\"\n           class=\"wpdtSimpleTable wpDataTable\"\n           data-column=\"7\"\n           data-rows=\"18\"\n           data-wpID=\"874\"\n           data-responsive=\"0\"\n           data-has-header=\"1\">\n\n                    <thead>        <tr class=\"wpdt-cell-row \" >\n                                <th class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"A1\"\n                    data-col-index=\"0\"\n                    data-row-index=\"0\"\n                    style=\" width:14.285714285714%;                    padding:10px;\n                    \"\n                    >\n                                        Operations                    <\/th>\n                                                <th class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"B1\"\n                    data-col-index=\"1\"\n                    data-row-index=\"0\"\n                    style=\" width:14.285714285714%;                    padding:10px;\n                    \"\n                    >\n                                        Tool Types                    <\/th>\n                                                <th class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"C1\"\n                    data-col-index=\"2\"\n                    data-row-index=\"0\"\n                    style=\" width:14.285714285714%;                    padding:10px;\n                    \"\n                    >\n                                        Tool Geometryand Set-Up                    <\/th>\n                                                <th class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"D1\"\n                    data-col-index=\"3\"\n                    data-row-index=\"0\"\n                    style=\" width:14.285714285714%;                    padding:10px;\n                    \"\n                    >\n                                        Speed                    <\/th>\n                                                <th class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"E1\"\n                    data-col-index=\"4\"\n                    data-row-index=\"0\"\n                    style=\" width:14.285714285714%;                    padding:10px;\n                    \"\n                    >\n                                        Feed                    <\/th>\n                                                <th class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"F1\"\n                    data-col-index=\"5\"\n                    data-row-index=\"0\"\n                    style=\" width:14.285714285714%;                    padding:10px;\n                    \"\n                    >\n                                        Depth of Cut                    <\/th>\n                                                <th class=\"wpdt-cell wpdt-bold wpdt-bc-063D71 wpdt-tc-FFFFFF\"\n                                            data-cell-id=\"G1\"\n                    data-col-index=\"6\"\n                    data-row-index=\"0\"\n                    style=\" width:14.285714285714%;                    padding:10px;\n                    \"\n                    >\n                                        Lubricant                    <\/th>\n                                        <\/tr>\n                    <tbody>        <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"A2\"\n                    data-col-index=\"0\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"B2\"\n                    data-col-index=\"1\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"C2\"\n                    data-col-index=\"2\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"D2\"\n                    data-col-index=\"3\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        surface ft.\/min*                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"E2\"\n                    data-col-index=\"4\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in**                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bold wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"F2\"\n                    data-col-index=\"5\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        in**                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-bc-EEEFF1\"\n                                            data-cell-id=\"G2\"\n                    data-col-index=\"6\"\n                    data-row-index=\"1\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell wpdt-wrap-text\"\n                                            data-cell-id=\"A3\"\n                    data-col-index=\"0\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Roughing with\u00a0severe interruptions; Turning or Facing                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B3\"\n                    data-col-index=\"1\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Carbide: C-2 or C-3grade                    <\/td>\n                                                <td class=\"wpdt-cell wpdt-wrap-text\"\n                                            data-cell-id=\"C3\"\n                    data-col-index=\"2\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">Negative rake square or trigon insert,&nbsp; 45&deg; SCEA<sup>1<\/sup>, 1\/16 in nose radius Tool holder: 5&deg; negative back rake, 5&deg; negative side rake<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D3\"\n                    data-col-index=\"3\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        30-50                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E3\"\n                    data-col-index=\"4\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.004-0.008per revolution                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F3\"\n                    data-col-index=\"5\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G3\"\n                    data-col-index=\"6\"\n                    data-row-index=\"2\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">Dry<sup>2<\/sup>, oil<sup>3<\/sup>, or water-based<sup>4,5<\/sup><\/div>                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A4\"\n                    data-col-index=\"0\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Normal roughing; Turning or Facing                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B4\"\n                    data-col-index=\"1\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        As above                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C4\"\n                    data-col-index=\"2\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        As above\u00a0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D4\"\n                    data-col-index=\"3\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">90 (80 for cobalt alloys)<sup>6<\/sup><\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E4\"\n                    data-col-index=\"4\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.010per revolution                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F4\"\n                    data-col-index=\"5\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <0.15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G4\"\n                    data-col-index=\"6\"\n                    data-row-index=\"3\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Dry, oil, or water-based                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A5\"\n                    data-col-index=\"0\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Finishing; Turning or Facing                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B5\"\n                    data-col-index=\"1\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        As above\u00a0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C5\"\n                    data-col-index=\"2\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">Positive rake square or trigon insert, if possible, 45&deg; SCEA<sup>1<\/sup>, 1\/32 in nose radius Tool holder: 5&deg; positive back rake, 5&deg; positive side rake<\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D5\"\n                    data-col-index=\"3\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        95-110 (90 for cobalt alloys)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E5\"\n                    data-col-index=\"4\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.005-0.007 per revolution                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F5\"\n                    data-col-index=\"5\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G5\"\n                    data-col-index=\"6\"\n                    data-row-index=\"4\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Dry or water-based                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A6\"\n                    data-col-index=\"0\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Rough Boring                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B6\"\n                    data-col-index=\"1\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        As Above                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C6\"\n                    data-col-index=\"2\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        If insert-type boring bar, use standard positive rake tools with largest possible SCEA\u00a0and 1\/16 in nose radius. \u00a0If brazed tool bar, grind 0\u00b0 back rake, 10\u00b0 positive side rake, 1\/32 in nose radius and largest possible SCEA                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D6\"\n                    data-col-index=\"3\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        70 (60 for cobalt alloys)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E6\"\n                    data-col-index=\"4\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.005-0.008 per revolution                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F6\"\n                    data-col-index=\"5\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.125                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G6\"\n                    data-col-index=\"6\"\n                    data-row-index=\"5\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Dry, oil, or water-based                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"3\"                     data-cell-id=\"A7\"\n                    data-col-index=\"0\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Finish Boring                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B7\"\n                    data-col-index=\"1\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        As Above                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C7\"\n                    data-col-index=\"2\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Use standard positive rake tools on insert-type bars. Grind brazed bars as for finish turning, except back rake may be best at 0\u00b0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D7\"\n                    data-col-index=\"3\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        95-110 (90 for cobalt alloys)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E7\"\n                    data-col-index=\"4\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.002-0.004 per revolution                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F7\"\n                    data-col-index=\"5\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.04                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G7\"\n                    data-col-index=\"6\"\n                    data-row-index=\"6\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Water-based                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B8\"\n                    data-col-index=\"1\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        <div data-type-content=\"wpdt-html-content\">High Speed Steel: M-2, M-7, or M-40&nbsp; series<sup>7<\/sup><\/div>                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C8\"\n                    data-col-index=\"2\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Radial and axial rake0\u00b0 to 10\u00b0 positive, 45\u00b0 corner angle, 10\u00b0 relief angle                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D8\"\n                    data-col-index=\"3\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20-30 (20-25 for cobalt alloys)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E8\"\n                    data-col-index=\"4\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.003-0.005 per tooth                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F8\"\n                    data-col-index=\"5\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G8\"\n                    data-col-index=\"6\"\n                    data-row-index=\"7\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Oil or water-based                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B9\"\n                    data-col-index=\"1\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Carbide: C-2 grade (marginal performance)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C9\"\n                    data-col-index=\"2\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Use positive axial and radial rake, 45\u00b0 corner angle, 10\u00b0 relief angle                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D9\"\n                    data-col-index=\"3\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50-60 (35-40 for cobalt alloys)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E9\"\n                    data-col-index=\"4\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        0.005-0.008per tooth (0.005 per tooth for cobalt alloys)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F9\"\n                    data-col-index=\"5\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G9\"\n                    data-col-index=\"6\"\n                    data-row-index=\"8\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Oil or water-based                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A10\"\n                    data-col-index=\"0\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        End Milling                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B10\"\n                    data-col-index=\"1\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        High Speed Steel: M-40 series or T-15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C10\"\n                    data-col-index=\"2\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        If possible, use short mills with four or more flutes\u00a0for rigidity                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D10\"\n                    data-col-index=\"3\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        20-25 (15-20 for cobalt alloys)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E10\"\n                    data-col-index=\"4\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Feed per tooth: \u00bc in dia. 0.002 \u00bd in dia. 0.002 \u00be in dia. 0.0031 in dia. 0.004(cobalt alloys: \u00bc in dia. 0.001 \u00bd in dia. 0.0015 \u00be in dia. 0.0021 in dia. 0.003)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F10\"\n                    data-col-index=\"5\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G10\"\n                    data-col-index=\"6\"\n                    data-row-index=\"9\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Oil or water-based                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B11\"\n                    data-col-index=\"1\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Carbide: C-2 grade\u00a0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C11\"\n                    data-col-index=\"2\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Use sharp tools with 4 or more flutes\u00a0and variable lead, if possible                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D11\"\n                    data-col-index=\"3\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Carbide: C-2 grade (marginal performance)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E11\"\n                    data-col-index=\"4\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Use positive axial and radial rake, 45\u00b0 corner angle, 10\u00b0 relief angle                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F11\"\n                    data-col-index=\"5\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G11\"\n                    data-col-index=\"6\"\n                    data-row-index=\"10\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Oil or water-based                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A12\"\n                    data-col-index=\"0\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Drilling                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B12\"\n                    data-col-index=\"1\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        High Speed Steel: M-33, M-40 series,\u00a0or T-15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C12\"\n                    data-col-index=\"2\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Use short, heavy-web drills\u00a0with 135\u00b0 crank shaft point; thinning of web at point may reduce thrust and aid chip\u00a0control                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D12\"\n                    data-col-index=\"3\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10-15 (7-10 for cobalt alloys) Maximum of\u00a0200 rpm for\u00bc in dia. drills or smaller                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E12\"\n                    data-col-index=\"4\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Feed per rev.: \u215b in dia. 0.001 \u00bc in dia. 0.002 \u00bd in dia. 0.003 \u00be in dia. 0.0051 in dia. 0.007(same for cobalt alloys) \u00a0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F12\"\n                    data-col-index=\"5\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G12\"\n                    data-col-index=\"6\"\n                    data-row-index=\"11\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Oil or water-based Use coolant feed drills if possible                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B13\"\n                    data-col-index=\"1\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Carbide :C-2 grade\u00a0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C13\"\n                    data-col-index=\"2\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Not recommended, but tipped drills may be successful on rigid set-ups if depth is not great. The web must be thinned to reduce thrust; use 135\u00b0 included angle on point Gun drill can be used.                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D13\"\n                    data-col-index=\"3\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        50\n(40 for cobalt\nalloys)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E13\"\n                    data-col-index=\"4\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        As above                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F13\"\n                    data-col-index=\"5\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G13\"\n                    data-col-index=\"6\"\n                    data-row-index=\"12\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Oil or water-based Coolant-fed, carbide-tipped  drills may be economical in some set-ups                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A14\"\n                    data-col-index=\"0\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Reaming                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B14\"\n                    data-col-index=\"1\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        High Speed Steel: M-33, M-40 series,\u00a0or T-15                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C14\"\n                    data-col-index=\"2\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Use 45\u00b0 corner angle, narrow primary land, and 10\u00b0 relief angle                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D14\"\n                    data-col-index=\"3\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        10-15 (8 for cobalt\u00a0alloys)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E14\"\n                    data-col-index=\"4\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Feed per rev.: \u00bd in dia. 0.0032 in dia. 0.008 (same for cobalt alloys) \u00a0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F14\"\n                    data-col-index=\"5\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G14\"\n                    data-col-index=\"6\"\n                    data-row-index=\"13\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Oil or water-based                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B15\"\n                    data-col-index=\"1\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Carbide: C-2 or C-3grade \u00a0                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C15\"\n                    data-col-index=\"2\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Tipped reamers recommended; solid reamers require very good set-up. Tool geometry same as above.                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D15\"\n                    data-col-index=\"3\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        40\n(20 for cobalt\nalloys)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E15\"\n                    data-col-index=\"4\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        As above                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F15\"\n                    data-col-index=\"5\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G15\"\n                    data-col-index=\"6\"\n                    data-row-index=\"14\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Oil or\nwater-based                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"1\"  rowspan=\"2\"                     data-cell-id=\"A16\"\n                    data-col-index=\"0\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Tapping                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B16\"\n                    data-col-index=\"1\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        High Speed Steel: M-1, M-7, or M-10                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C16\"\n                    data-col-index=\"2\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Use two flute, spiral point, plug tap 0\u00b0 to 10\u00b0 hook angles. Nitrided surface may be helpful by increasing wear resistance, but may result in chipping orbreakage Tap drill for 60-65% thread if possible, to increase tool life.                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D16\"\n                    data-col-index=\"3\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        7 (same for cobalt alloys)                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E16\"\n                    data-col-index=\"4\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F16\"\n                    data-col-index=\"5\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G16\"\n                    data-col-index=\"6\"\n                    data-row-index=\"15\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Use best possible tapping compound; sulfo-chlorinated oil-base preferred                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                            <td class=\"wpdt-cell \"\n                                            data-cell-id=\"B17\"\n                    data-col-index=\"1\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Carbide: not recommended                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"C17\"\n                    data-col-index=\"2\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"D17\"\n                    data-col-index=\"3\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"E17\"\n                    data-col-index=\"4\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"F17\"\n                    data-col-index=\"5\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"G17\"\n                    data-col-index=\"6\"\n                    data-row-index=\"16\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        -                    <\/td>\n                                        <\/tr>\n                            <tr class=\"wpdt-cell-row \" >\n                                <td class=\"wpdt-cell \"\n                                            data-cell-id=\"A18\"\n                    data-col-index=\"0\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        Electrical\nDischarge\nMachining                    <\/td>\n                                                <td class=\"wpdt-cell  wpdt-merged-cell \"\n                     colspan=\"6\"  rowspan=\"1\"                     data-cell-id=\"B18\"\n                    data-col-index=\"1\"\n                    data-row-index=\"17\"\n                    style=\"                    padding:10px;\n                    \"\n                    >\n                                        HAYNES<sup>\u00ae<\/sup> and HASTELLOY<sup>\u00ae<\/sup> alloys can be readily cut using any conventional\nElectrical discharge machining (EDM) system, or by wire EDM                    <\/td>\n                                                                                                    <\/tr>\n                    <\/table>\n<\/div><style id='wpdt-custom-style-874'>\n.wpdt-bc-063D71 { background-color: #063D71 !important;}\n.wpdt-tc-FFFFFF { color: #FFFFFF !important;}\n.wpdt-bc-EEEFF1 { background-color: #EEEFF1 !important;}\n<\/style>\n\n\n\n\n<p class=\"wp-block-paragraph\"><strong>General note:<\/strong>&nbsp;Use high pressure coolant systems and through the tool coolant, when possible.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">*To convert to surface m\/min, multiply by 0.305<br>**To convert from in to mm, multiply by 25.4<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><sup>1<\/sup>SCEA = side cutting edge angle, or lead angle of the tool<br><sup>2<\/sup>At any point where dry cutting is recommended, an air jet directed at the tool may provide a substantial increase in tool life<br><sup>3<\/sup>Oil coolants should be premium quality, sulfo-chlorinated oils, with extreme pressure additives; a viscosity of 50 to 125 SSU at 100\u00b0F (38\u00b0C) is standard<br><sup>4<\/sup>Water-based coolants should consist of a 15:1 mixture of water and either a premium quality, sulfo-chlorinated, water-soluble oil or a chemical emulsion, with extreme pressure additives<br><sup>5<\/sup>Water-based coolants may cause chipping or rapid failure of carbide tools in interrupted cuts<br><sup>6<\/sup>Depending upon the rigidity of the set-up<br><sup>7<\/sup>M-40 series high speed steels include M-41 through M-46 at time of writing; others may be added and should be equally suitable<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Applicable to:<\/strong><br><strong>Wear &amp; Corrosion-resistant Alloy<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">ULTIMET<sup>\u00ae<\/sup>&nbsp;alloy can be successfully turned, drilled, and milled if appropriate tooling and parameters are employed. However, the alloy possesses high strength and work hardens rapidly. Machining guidelines specific to ULTIMET<sup>\u00ae<\/sup>&nbsp;alloy are as follows:<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Turning (ULTIMET<sup>\u00ae<\/sup>&nbsp;alloy)<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Carbide (not high speed steel) tools are recommended.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Surface speed: 60-70 surface ft.\/min (0.30-0.35 m\/s).<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Feed rate: 0.005-0.010 in (0.13-0.25 mm).<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Depth of cut for roughing: 0.05-0.10 in (1.3-2.5 mm).<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Depth of cut for finishing: 0.010-0.015 in (0.25-0.38 mm).<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Drilling (ULTIMET<sup>\u00ae<\/sup>&nbsp;alloy)<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Carbide tipped or high speed steel drills are recommended.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Surface speed: 30-35 surface ft.\/min (0.15-0.18 m\/s) for carbide tipped drills; 8-10 surface ft\/min (0.04-0.05 m\/s) for high speed steel drills.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Feed rate: 0.004 in (0.1 mm) per revolution for 0.25 in (6.4 mm) diameter and greater.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">135\u00b0 included angle on point.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Milling (ULTIMET<sup>\u00ae<\/sup>&nbsp;alloy)<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Carbide (not high speed steel) end mills are recommended.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Surface speed: 25-30 surface ft\/min (0.13-0.15 m\/s).<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Feed per tooth: 0.002 in (0.05 mm) for cutter diameters below 0.75 in (19 mm); 0.003 in (0.08 mm) for cutter diameters above 0.75 in (19 mm).<\/p>\n","protected":false},"excerpt":{"rendered":"<p>Recommended Tools and Machining Parameters Applicable to:Corrosion-resistant AlloysHigh-temperature Alloys Be aware that the cobalt-base alloys in these categories (25 and 188) can require different feeds and speeds (as noted in the table) than the nickel- and iron-based alloys. General note:&nbsp;Use high pressure coolant systems and through the tool coolant, when possible. *To convert to surface [\u2026]<\/p>\n","protected":false},"author":2,"featured_media":4483,"parent":55,"menu_order":4,"template":"","meta":{"_acf_changed":false,"_searchwp_excluded":"","inline_featured_image":false,"footnotes":""},"class_list":["post-108","alloys","type-alloys","status-publish","has-post-thumbnail","hentry"],"acf":[],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v27.8 (Yoast SEO v28.6) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Machining - Haynes International machining, alloy machining, CNC, cutting<\/title>\n<meta name=\"description\" content=\"Discover Haynes International&#039;s precision machining services with expert CNC turning, milling, drilling, and intricate machining for high-performance nickel, cobalt, titanium, and specialty alloys. Engineered for tight tolerances and critical applications in aerospace, energy, medical, and industrial sectors.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/\" \/>\n<meta property=\"og:locale\" content=\"en_US\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Machining\" \/>\n<meta property=\"og:description\" content=\"Discover Haynes International&#039;s precision machining services with expert CNC turning, milling, drilling, and intricate machining for high-performance nickel, cobalt, titanium, and specialty alloys. Engineered for tight tolerances and critical applications in aerospace, energy, medical, and industrial sectors.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/\" \/>\n<meta property=\"og:site_name\" content=\"Haynes International\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/HaynesInternationalInc\/\" \/>\n<meta property=\"article:modified_time\" content=\"2025-07-18T14:29:05+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/06\/shutterstock_1014005701.jpg?fit=1183%2C754&ssl=1\" \/>\n\t<meta property=\"og:image:width\" content=\"1183\" \/>\n\t<meta property=\"og:image:height\" content=\"754\" \/>\n\t<meta property=\"og:image:type\" content=\"image\/jpeg\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:site\" content=\"@HaynesIntl\" \/>\n<meta name=\"twitter:label1\" content=\"Est. reading time\" \/>\n\t<meta name=\"twitter:data1\" content=\"2 minutes\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/welding-and-fabrication\\\/machining\\\/\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/welding-and-fabrication\\\/machining\\\/\",\"name\":\"Machining - Haynes International machining, alloy machining, CNC, cutting\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/welding-and-fabrication\\\/machining\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/welding-and-fabrication\\\/machining\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/06\\\/shutterstock_1014005701.jpg?fit=1183%2C754&ssl=1\",\"datePublished\":\"2024-06-29T01:44:39+00:00\",\"dateModified\":\"2025-07-18T14:29:05+00:00\",\"description\":\"Discover Haynes International's precision machining services with expert CNC turning, milling, drilling, and intricate machining for high-performance nickel, cobalt, titanium, and specialty alloys. Engineered for tight tolerances and critical applications in aerospace, energy, medical, and industrial sectors.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/welding-and-fabrication\\\/machining\\\/#breadcrumb\"},\"inLanguage\":\"en-US\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/welding-and-fabrication\\\/machining\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"en-US\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/welding-and-fabrication\\\/machining\\\/#primaryimage\",\"url\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/06\\\/shutterstock_1014005701.jpg?fit=1183%2C754&ssl=1\",\"contentUrl\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/06\\\/shutterstock_1014005701.jpg?fit=1183%2C754&ssl=1\",\"width\":1183,\"height\":754},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/welding-and-fabrication\\\/machining\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Welding and Fabrication\",\"item\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/alloys\\\/welding-and-fabrication\\\/\"},{\"@type\":\"ListItem\",\"position\":3,\"name\":\"Machining\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#website\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\",\"name\":\"Haynes International\",\"description\":\"The Home of HASTELLOY\u00ae and HAYNES\u00ae high-performance alloys\",\"publisher\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"en-US\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#organization\",\"name\":\"Haynes International\",\"url\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"en-US\",\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/07\\\/logo.webp?fit=484%2C188&ssl=1\",\"contentUrl\":\"https:\\\/\\\/i0.wp.com\\\/haynesintl.com\\\/wp-content\\\/uploads\\\/2024\\\/07\\\/logo.webp?fit=484%2C188&ssl=1\",\"width\":484,\"height\":188,\"caption\":\"Haynes International\"},\"image\":{\"@id\":\"https:\\\/\\\/haynesintl.com\\\/en\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/HaynesInternationalInc\\\/\",\"https:\\\/\\\/x.com\\\/HaynesIntl\",\"https:\\\/\\\/www.instagram.com\\\/haynesinternational\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/company\\\/haynes-international\\\/\"]}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Machining - Haynes International machining, alloy machining, CNC, cutting","description":"Discover Haynes International's precision machining services with expert CNC turning, milling, drilling, and intricate machining for high-performance nickel, cobalt, titanium, and specialty alloys. Engineered for tight tolerances and critical applications in aerospace, energy, medical, and industrial sectors.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/","og_locale":"en_US","og_type":"article","og_title":"Machining","og_description":"Discover Haynes International's precision machining services with expert CNC turning, milling, drilling, and intricate machining for high-performance nickel, cobalt, titanium, and specialty alloys. Engineered for tight tolerances and critical applications in aerospace, energy, medical, and industrial sectors.","og_url":"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/","og_site_name":"Haynes International","article_publisher":"https:\/\/www.facebook.com\/HaynesInternationalInc\/","article_modified_time":"2025-07-18T14:29:05+00:00","og_image":[{"width":1183,"height":754,"url":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/06\/shutterstock_1014005701.jpg?fit=1183%2C754&ssl=1","type":"image\/jpeg"}],"twitter_card":"summary_large_image","twitter_site":"@HaynesIntl","twitter_misc":{"Est. reading time":"2 minutes"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"WebPage","@id":"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/","url":"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/","name":"Machining - Haynes International machining, alloy machining, CNC, cutting","isPartOf":{"@id":"https:\/\/haynesintl.com\/en\/#website"},"primaryImageOfPage":{"@id":"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/#primaryimage"},"image":{"@id":"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/#primaryimage"},"thumbnailUrl":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/06\/shutterstock_1014005701.jpg?fit=1183%2C754&ssl=1","datePublished":"2024-06-29T01:44:39+00:00","dateModified":"2025-07-18T14:29:05+00:00","description":"Discover Haynes International's precision machining services with expert CNC turning, milling, drilling, and intricate machining for high-performance nickel, cobalt, titanium, and specialty alloys. Engineered for tight tolerances and critical applications in aerospace, energy, medical, and industrial sectors.","breadcrumb":{"@id":"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/#breadcrumb"},"inLanguage":"en-US","potentialAction":[{"@type":"ReadAction","target":["https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/"]}]},{"@type":"ImageObject","inLanguage":"en-US","@id":"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/#primaryimage","url":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/06\/shutterstock_1014005701.jpg?fit=1183%2C754&ssl=1","contentUrl":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/06\/shutterstock_1014005701.jpg?fit=1183%2C754&ssl=1","width":1183,"height":754},{"@type":"BreadcrumbList","@id":"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/machining\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/haynesintl.com\/en\/"},{"@type":"ListItem","position":2,"name":"Welding and Fabrication","item":"https:\/\/haynesintl.com\/en\/alloys\/welding-and-fabrication\/"},{"@type":"ListItem","position":3,"name":"Machining"}]},{"@type":"WebSite","@id":"https:\/\/haynesintl.com\/en\/#website","url":"https:\/\/haynesintl.com\/en\/","name":"Haynes International","description":"The Home of HASTELLOY\u00ae and HAYNES\u00ae high-performance alloys","publisher":{"@id":"https:\/\/haynesintl.com\/en\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/haynesintl.com\/en\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"en-US"},{"@type":"Organization","@id":"https:\/\/haynesintl.com\/en\/#organization","name":"Haynes International","url":"https:\/\/haynesintl.com\/en\/","logo":{"@type":"ImageObject","inLanguage":"en-US","@id":"https:\/\/haynesintl.com\/en\/#\/schema\/logo\/image\/","url":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/07\/logo.webp?fit=484%2C188&ssl=1","contentUrl":"https:\/\/i0.wp.com\/haynesintl.com\/wp-content\/uploads\/2024\/07\/logo.webp?fit=484%2C188&ssl=1","width":484,"height":188,"caption":"Haynes International"},"image":{"@id":"https:\/\/haynesintl.com\/en\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/HaynesInternationalInc\/","https:\/\/x.com\/HaynesIntl","https:\/\/www.instagram.com\/haynesinternational\/","https:\/\/www.linkedin.com\/company\/haynes-international\/"]}]}},"jetpack_sharing_enabled":true,"_links":{"self":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys\/108","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys"}],"about":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/types\/alloys"}],"author":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/users\/2"}],"version-history":[{"count":3,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys\/108\/revisions"}],"predecessor-version":[{"id":6832,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys\/108\/revisions\/6832"}],"up":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/alloys\/55"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/media\/4483"}],"wp:attachment":[{"href":"https:\/\/haynesintl.com\/en\/wp-json\/wp\/v2\/media?parent=108"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}