Tensile Data, Plate
Test Temperature |
Ultimate Tensile Strength |
0.2% Yield Strength |
Elongation |
°F |
°C |
ksi |
MPa |
ksi |
MPa |
% |
RT |
RT |
200.5 |
1382 |
167.8 |
1157 |
20.6 |
800 |
427 |
173.1 |
1193 |
149.0 |
1027 |
22.6 |
1000 |
538 |
170.2 |
1173 |
145.9 |
1006 |
21.8 |
1200 |
649 |
162.5 |
1120 |
139.9 |
965 |
25.1 |
1400 |
760 |
117.3 |
809 |
104.9 |
723 |
12.1 |
1600 |
871 |
42.2 |
291 |
34.3 |
236 |
68.0 |
1800 |
982 |
14.1 |
97 |
9.6 |
66 |
129.9 |
Mill Annealed + 1325°F/8h/Furnace Cool to 1150°F/8h/Air Cool
Total time: 18 hours
RT= Room Temperature
Tensile Data, Sheet
Test Temperature |
Ultimate Tensile Strength |
0.2% Yield Strength |
Elongation |
°F |
°C |
ksi |
MPa |
ksi |
MPa |
% |
RT |
RT |
203.6 |
1404 |
174.7 |
1205 |
18.4 |
800 |
427 |
176.2 |
1215 |
155.4 |
1071 |
21.3 |
1000 |
538 |
172.3 |
1188 |
150.2 |
1036 |
20.7 |
1200 |
649 |
164.1 |
1131 |
144.3 |
995 |
16.3 |
1400 |
760 |
114.8 |
792 |
103.8 |
716 |
6.9 |
1600 |
871 |
39.9 |
275 |
34.0 |
234 |
81.8 |
1800 |
982 |
13.7 |
94 |
9.7 |
67 |
175.6 |
Mill Annealed + 1325°F/8h/Furnace Cool to 1150°F/8h/Air Cool
Total time: 18 hours