Static Oxidation Testing

Environment: Flowing Air
Test Duration: 1,008 h
Number of Cycles: 6
Cycle Length: 168 h
Temperatures: 1600, 1700, 1800°F (871, 927, 982°C)
Metal Loss = (A-B)/2
Average Internal Penetration = C
Maximum Internal Penetration = D
Average Metal Affected = Metal Loss + Average Internal Penetration
Maximum Metal Affected = Metal Loss + Maximum Internal Penetration

282 - metal loss

Comparative Oxidation Resistance in Flowing Air, 1008 Hours


Alloy
1600°F (871°C) 1700°F (927°C) 1800°F (982°C)
Metal Loss
Avg. Met. Aff.
Metal Loss
Avg. Met. Aff.
Metal Loss
Avg. Met. Aff.
mils μm mils μm mils μm mils μm mils μm mils μm
263 0.1 3 0.4 10 0.2 5 0.7 18 0.9 23 5.0 127
282® 0.2 5 0.6 15 0.1 3 1.1 28 0.2 5 1.8 46
R‐41 0.2 5 0.8 20 0.2 5 1.5 38 0.2 5 2.9 74
Waspaloy 0.3 8 1.4 36 0.3 8 3.4 86 0.7 18 5.0 127

Dynamic Oxidation Testing (Burner Rig)

Burner rig oxidation tests were conducted by exposing, in a rotating holder, samples 0.375 inch x 2.5 inches x thickness (9.5mm x 64mm x thickness) to the products of combustion of fuel oil (2 parts No. 1 and 1 part No. 2), burned at an air to fuel ratio of about 50:1. The gas velocity was about 0.3 mach. Samples were automatically removed from the gas stream every 30 minutes and fan cooled to less than 500°F (260°C) and then reinserted into the flame tunnel.

Alloy 1600°F (871°C), 1000 hours, 30 minute cycles 1800°F (982°C), 1000 hours, 30 minute cycles
Metal Loss,
Avg. Met. Aff.
Metal Loss,
Avg. Met. Aff.
mils μm mils μm mils μm mils μm
263 1.4 36 4.0 102 12.5 318 16.1 409
282® 1.8 46 4.2 107 8.0 203 13.0 330
Waspaloy 1.9 48 4.3 109 9.5 241 13.6 345
R‐41 1.2 30 4.4 112 5.8 147 12.1 307