Haynes International
Investor Relations
Customer Portal
English
日本語
中文
español
800.354.0806
765.456.6012
The Home of HASTELLOY® and
HAYNES® Alloys
Our Company
Company Overview
Locations and Directions
Corporate Governance
Corporate Governance Guidelines
Corporate Policies
Human Trafficking Policy and Disclosure Statement
Human Rights Policy
Insider Trading Policy
Conflicts Minerals Policy
Gift Policy
Cancellation Policy
Anti-Harassment Policy
Anti-Corruption Policy
Health, Safety, Environmental, and Quality Policy
Energy Policy
Code of Business Conduct and Ethics
Code of Business Conduct and Ethics, English
Code of Business Conduct and Ethics, Chinese
Code of Business Conduct and Ethics, French
Code of Business Conduct and Ethics, German
Code of Conduct for Haynes Suppliers and Third Party Intermediaries
EthicsPoint Whistleblower Hotline/ Code of Business Conduct
Compliance with the Code of Business Conduct and Ethics
Directors and Executive Officers
Composition of Board Committees
Board Committee Charters
Sustainability
Environmental
Social
Governance
Code of Business Conduct and Ethics Compliance
Sustainability Steering Committee
Our Positive Impact
Health, Safety, Environmental, and Quality
Health, Safety, Environmental, and Quality Policy
MSDS/Safety Data Sheets
Safety Data Sheets, English
Safety Data Sheets, Chinese
Safety Data Sheets, Czech
Safety Data Sheets, French
Safety Data Sheets, German
Safety Data Sheets, Italian
Safety Data Sheets, Japanese
Safety Data Sheets, Korean
Safety Data Sheets, Spanish
Energy Policy
Accreditations and Approvals
REACh
Trademarks
Our Heritage
Our Founder, Elwood Haynes
Our Company History
Our Milestones
Our Contributions to History
Careers
News
Markets
Aerospace
Power Generation
Chemical Processing
Emerging Technologies
Other Markets
Alloys
Alloy Portfolio
High-temperature Alloys
HAYNES® 25 alloy
HAYNES® 75 alloy
HAYNES® 188 alloy
HAYNES® 214® alloy
HAYNES® 230® alloy
HAYNES® 233™ alloy
HAYNES® 242® alloy
HAYNES® 244® alloy
HAYNES® 263 alloy
HAYNES® 282® alloy
HAYNES® 556® alloy
HAYNES® 617 alloy
HAYNES® 625 alloy
HAYNES® 625SQ® alloy
HAYNES® 718 alloy
HAYNES® HR-120® alloy
HAYNES® HR-160® alloy
HAYNES® HR-224® alloy
HAYNES® HR-235® alloy
MULTIMET® alloy
HAYNES® NS-163® alloy
HAYNES® R-41 alloy
HASTELLOY® S alloy
HASTELLOY® W alloy
HAYNES® Waspaloy alloy
HASTELLOY® X alloy
HAYNES® X-750 alloy
Corrosion-resistant Alloys
HASTELLOY® B-3® alloy
HASTELLOY® C-4 alloy
HASTELLOY® C-22® alloy
HASTELLOY® C-22HS® alloy
HASTELLOY® C-276 alloy
HASTELLOY® C-2000® alloy
HASTELLOY® G-30® alloy
HASTELLOY® G-35® alloy
HASTELLOY® HYBRID-BC1® alloy
HASTELLOY® N alloy
ULTIMET® alloy
Titanium Alloy
HAYNES® Ti-3Al-2.5V alloy
Alloy Nominal Compositions
Product Forms
Sheet and Plate
Wire and Welding
TIG (GTAW) and MIG (GMAW) Filler Metal Products
Coated Electrodes
Thermal Spray
Medical Wire
Standard Sizes
Small Bar
Welding and Joining Guidelines
MSDS/Safety Data Sheets
Welding SmartGuide
Wire Products Brochure
Pipe and Tubing
Corrosion-resistant alloys
High-temperature alloys
Titanium alloy
Tubular Products Brochure
Bar and Billet
Fittings and Flanges
Welding and Fabrication
Welding and Fabrication Overview
Wire and Welding Product Forms
Hot-working
Cold-working
Welding and Joining
Welding and Joining Guidelines
Weld Joint Design
Weld Joint Preparation
Temperature Control and Heat Treatment of Weldments
Welding Defects
Postweld Inspection and Repair
Gas Tungsten Arc Welding (GTAW / “TIG”)
Gas Metal Arc Welding (GMAW / “MIG”)
Shielded Metal Arc Welding (SMAW / “Stick”)
Plasma Arc Welding (PAW)
Electron Beam Welding (EBW) and Laser Beam Welding (LBW)
Brazing and Soldering
Welding and Joining Brochure
Welding SmartGuide
Heat Treatment
Machining
Grinding
Descaling and Pickling
Welding SmartGuide
Welding and Fabrication Brochure
Corrosion Guide
Alloy Backgrounds
Alloy Groups
Metallurgy
Corrosive Environments
Wear Background
Abrasion
Erosion
Metal‐to‐Metal Sliding Wear
Corrosion Alloy Manual
Alloy Innovation
Alloy Development
Alloy Manufacturing
Alloy Technical Support
Specifications and Codes
Accreditations and Approvals
MSDS/Safety Data Sheets
Safety Data Sheets, English
Safety Data Sheets, Chinese
Safety Data Sheets, Czech
Safety Data Sheets, French
Safety Data Sheets, German
Safety Data Sheets, Italian
Safety Data Sheets, Japanese
Safety Data Sheets, Korean
Safety Data Sheets, Spanish
Trademarks
Technical Library
Sales and Service
Sales and Service
Sales Office and Service Center Locations
Request for Quote
Terms and Conditions of Sale
Cancellation Policy
Export Compliance Policy Letter
Due Diligence
Incoterms®
Alloys and Products Brochure
Processing Capabilities
Abrasive Saw Cutting
Bar Saw Cutting
Laser Cutting
Near-net Shaped Cut Parts
Plasma Cutting
Precision Shearing
Virtek® Laser QC®
Waterjet Cutting
Contact
Sales
Technical Support
Investor Relations
Careers
General Information
HAYNES® 556® alloy
Home
/
Alloys
/
Alloy Portfolio
/
High-temperature Alloys
/
HAYNES® 556® alloy
/
Physical Properties
ASP.sfctrlpresentation_openaccessdataprovider_7b98424546ba62e18cdfff0000376e70_ascx
HAYNES® 556® alloy
Principal Features
Nominal Composition
Sulfidation Resistance
Carburization Resistance
Oxidation Resistance
Resistance to Chlorine-Bearing Environments
Other Environments
Physical Properties
Applications
Tensile Properties
Creep and Rupture Properties
Impact Properties
Thermal Stability
Fabrication Characteristics
Welding
Specifications and Codes
Disclaimer
Alloy Brochure
Principal Features
Nominal Composition
Sulfidation Resistance
Carburization Resistance
Oxidation Resistance
Resistance to Chlorine-Bearing Environments
Other Environments
Physical Properties
Applications
Tensile Properties
Creep and Rupture Properties
Impact Properties
Thermal Stability
Fabrication Characteristics
Welding
Specifications and Codes
Disclaimer
Alloy Brochure
Principal Features
Nominal Composition
Sulfidation Resistance
Carburization Resistance
Oxidation Resistance
Resistance to Chlorine-Bearing Environments
Other Environments
Physical Properties
Applications
Tensile Properties
Creep and Rupture Properties
Impact Properties
Thermal Stability
Fabrication Characteristics
Welding
Specifications and Codes
Disclaimer
Alloy Brochure
Physical Properties
Physical Property
British Units
Metric Units
Density
RT
0.297 lb/in
3
RT
8.23 g/cm
3
Melting Temperature
2425-2580°F
-
1330-1415°C
-
Electrical Resistivity
RT
35.7 µohm-in
RT
95.2 µohm-cm
200°F
38.7 µohm-in
100°C
98.6 µohm-cm
400°F
40.5 µohm-in
200°C
102.6 µohm-cm
600°F
42.1 µohm-in
300°C
106.5 µohm-cm
800°F
43.5 µohm-in
400°C
109.5 µohm-cm
1000°F
44.7 µohm-in
500°C
112.5 µohm-cm
1200°F
45.7 µohm-in
600°C
115.1 µohm-cm
1400°F
46.6 µohm-in
700°C
117.2 µohm-cm
1600°F
47.3 µohm-in
800°C
119.0 µohm-cm
1800°F
48.0 µohm-in
900°C
120.7 µohm-cm
2000°F
48.6 µohm-in
1000°C
122.3 µohm-cm
-
-
1100°C
123.7 µohm-cm
Thermal Diffusivity
RT
4.5 x 10
-3
in
2
/s
RT
28.7 x 10
-3
cm
2
/s
200°F
4.8 x 10
-3
in
2
/s
100°C
31.2 x 10
-3
cm
2
/s
400°F
5.3 x 10
-3
in
2
/s
200°C
34.2 x 10
-3
cm
2
/s
600°F
5.8 x 10
-3
in
2
/s
300°C
37.0 x 10
-3
cm
2
/s
800°F
6.3 x 10
-3
in
2
/s
400°C
39.7 x 10
-3
cm
2
/s
1000°F
6.7 x 10
-3
in
2
/s
500°C
42.3 x 10
-3
cm
2
/s
1200°F
7.1 x 10
-3
in
2
/s
600°C
44.8 x 10
-3
cm
2
/s
1400°F
7.5 x 10
-3
in
2
/s
700°C
47.0 x 10
-3
cm
2
/s
1600°F
7.7 x 10
-3
in
2
/s
800°C
48.8 x 10
-3
cm
2
/s
1800°F
8.0 x 10
-3
in
2
/s
900°C
50.3 x 10
-3
cm
2
/s
2000°F
8.2 x 10
-3
in
2
/s
1000°C
51.6 x 10
-3
cm
2
/s
-
-
1100°C
52.8 x 10
-3
cm
2
/s
Thermal Conductivity
RT
77 Btu-in/ft
2
-hr-°F
RT
11.1 W/m-°C
200°F
90 Btu-in/ft
2
-hr-°F
100°C
13.1 W/m-°C
400°F
107 Btu-in/ft
2
-hr-°F
200°C
15.4 W/m-°C
600°F
122 Btu-in/ft
2
-hr-°F
300°C
17.3 W/m-°C
800°F
135 Btu-in/ft
2
-hr-°F
400°C
19.0 W/m-°C
1000°F
148 Btu-in/ft
2
-hr-°F
500°C
20.8 W/m-°C
1200°F
160 Btu-in/ft
2
-hr-°F
600°C
22.4 W/m-°C
1400°F
173 Btu-in/ft
2
-hr-°F
700°C
24.0 W/m-°C
1600°F
185 Btu-in/ft
2
-hr-°F
800°C
25.5 W/m-°C
1800°F
197 Btu-in/ft
2
-hr-°F
900°C
27.2 W/m-°C
2000°F
210 Btu-in/ft
2
-hr-°F
1000°C
28.9 W/m-°C
-
-
1100°C
30.4 W/m-°C
Specific Heat
RT
0.111 Btu/lb-°F
RT
464 J/kg·°C
200°F
0.113 Btu/lb-°F
100°C
475 J/kg·°C
400°F
0.118 Btu/lb-°F
200°C
493 J/kg·°C
600°F
0.122 Btu/lb-°F
300°C
508 J/kg·°C
800°F
0.126 Btu/lb-°F
400°C
523 J/kg·°C
1000°F
0.130 Btu/lb-°F
500°C
538 J/kg·°C
1200°F
0.133 Btu/lb-°F
600°C
552 J/kg·°C
1400°F
0.135 Btu/lb-°F
700°C
561 J/kg·°C
1600°F
0.140 Btu/lb-°F
800°C
570 J/kg·°C
1800°F
0.147 Btu/lb-°F
900°C
595 J/kg·°C
2000°F
0.152 Btu/lb-°F
1000°C
618 J/kg·°C
-
-
1100°C
638 J/kg·°C
Mean Coefficient of
Thermal Expansion
70-200°F
8.1 µin/in -°F
25-100°C
14.7 x 10
-6
m/m·°C
70-400°F
8.2 µin/in -°F
25-200°C
14.9 x 10
-6
m/m·°C
70-600°F
8.4 µin/in -°F
25-300°C
15.1 x 10
-6
m/m·°C
70-800°F
8.6 µin/in -°F
25-400°C
15.4 x 10
-6
m/m·°C
70-1000°F
8.8 µin/in -°F
25-500°C
15.7 x 10
-6
m/m·°C
70-1200°F
9.0 µin/in -°F
25-600°C
16.1 x 10
-6
m/m·°C
70-1400°F
9.2 µin/in -°F
25-700°C
16.4 x 10
-6
m/m·°C
70-1600°F
9.4 µin/in -°F
25-800°C
16.7 x 10
-6
m/m·°C
70-1800°F
9.5 µin/in -°F
25-900°C
17.0 x 10
-6
m/m·°C
70-2000°F
9.6 µin/in -°F
25-1000°C
17.1 x 10
-6
m/m·°C
-
-
25-1100°C
17.1 x 10
-6
m/m·°C
Dynamic Modulus
of Elasticity
RT
29.7 x 10
6
psi
RT
205 GPa
200°F
29.1 x 10
6
psi
100°C
200 GPa
400°F
28.2 x 10
6
psi
200°C
195 GPa
600°F
26.9 x 10
6
psi
300°C
187 GPa
800°F
25.6 x 10
6
psi
400°C
179 GPa
1000°F
24.4 x 10
6
psi
500°C
172 GPa
1200°F
23.1 x 10
6
psi
600°C
164 GPa
1400°F
21.8 x 10
6
psi
700°C
155 GPa
1600°F
20.9 x 10
6
psi
800°C
148 Gpa
1800°F
20.1 x 10
6
psi
900°C
143 Gpa
-
-
1000°C
138 Gpa
RT= Room Temperature
Print Page
Download Page
Typical Physical Properties