Haynes International
Investor Relations
Customer Portal
English
日本語
中文
español
800.354.0806
765.456.6012
The Home of HASTELLOY® and HAYNES® Alloys
When autocomplete results are available use up and down arrows to review and enter to select.
Our Company
Company Overview
Locations and Directions
Investor Relations
Corporate Governance
Corporate Policies
Human Trafficking Policy
Human Rights Policy
Insider Trading Policy
Conflicts Minerals Policy
Gift Policy
Cancellation Policy
Anti-Harassment Policy
Anti-Corruption Policy
Health, Safety, Environmental, and Quality Policy
Energy Policy
Code of Business Conduct and Ethics
Code of Business Conduct and Ethics, English
Code of Business Conduct and Ethics, Chinese
Code of Business Conduct and Ethics, French
Code of Business Conduct and Ethics, German
Suppliers and Third Party Intermediaries
EthicsPoint Whistleblower Hotline
Conduct and Ethics Compliance
Directors and Executive Officers
Composition of Board Committees
Board Committee Charters
Corporate Governance Guidelines
Sustainability
Environmental
Social
Governance
Our Positive Impact
Health, Safety, Environmental, and Quality
Health, Safety, Environmental, and Quality Policy
MSDS/Safety Data Sheets
Safety Data Sheets, English
Safety Data Sheets, Chinese
Safety Data Sheets, Czech
Safety Data Sheets, French
Safety Data Sheets, German
Safety Data Sheets, Italian
Safety Data Sheets, Japanese
Safety Data Sheets, Korean
Safety Data Sheets, Spanish
Energy Policy
Accreditations and Approvals
REACh
Trademarks
Our Heritage
Our Founder, Elwood Haynes
Our Company History
Our Milestones
Our Contributions to History
Careers
News
Markets
Aerospace
Power Generation
Chemical Processing
Emerging Technologies
Other Markets
Alloys
Alloy Portfolio
High-temperature Alloys
HAYNES® 25 alloy
HAYNES® 75 alloy
HAYNES® 188 alloy
HAYNES® 214® alloy
HAYNES® 230® alloy
HAYNES® 233™ alloy
HAYNES® 242® alloy
HAYNES® 244® alloy
HAYNES® 263 alloy
HAYNES® 282® alloy
HAYNES® 556® alloy
HAYNES® 617 alloy
HAYNES® 625 alloy
HAYNES® 625SQ® alloy
HAYNES® 718 alloy
HAYNES® HR-120® alloy
HAYNES® HR-160® alloy
HAYNES® HR-224® alloy
HAYNES® HR-235® alloy
MULTIMET® alloy
HAYNES® NS-163® alloy
HAYNES® R-41 alloy
HASTELLOY® S alloy
HASTELLOY® W alloy
HAYNES® Waspaloy alloy
HASTELLOY® X alloy
HAYNES® X-750 alloy
Corrosion-resistant Alloys
HASTELLOY® B-3® alloy
HASTELLOY® C-4 alloy
HASTELLOY® C-22® alloy
HASTELLOY® C-22HS® alloy
HASTELLOY® C-276 alloy
HASTELLOY® C-2000® alloy
HASTELLOY® G-30® alloy
HASTELLOY® G-35® alloy
HASTELLOY® HYBRID-BC1® alloy
HASTELLOY® N alloy
ULTIMET® alloy
Titanium Alloy
HAYNES® Ti-3Al-2.5V alloy
Alloy Nominal Compositions
Product Forms
Sheet and Plate
Wire and Welding
TIG (GTAW) and MIG (GMAW) Filler Metal Products
Coated Electrodes
Thermal Spray
Medical Wire
Standard Sizes
Small Bar
Welding and Joining Guidelines
MSDS/Safety Data Sheets
Welding SmartGuide
Wire Products Brochure
Pipe and Tubing
Corrosion-resistant alloys
High-temperature alloys
Titanium alloy
Tubular Products Brochure
Bar and Billet
Fittings and Flanges
Welding and Fabrication
Welding and Fabrication Overview
Wire and Welding Product Forms
Hot-working
Cold-working
Welding and Joining
Welding and Joining Guidelines
Weld Joint Design
Weld Joint Preparation
Temperature Control and Heat Treatment of Weldments
Welding Defects
Postweld Inspection and Repair
Gas Tungsten Arc Welding (GTAW / “TIG”)
Gas Metal Arc Welding (GMAW / “MIG”)
Shielded Metal Arc Welding (SMAW / “Stick”)
Plasma Arc Welding (PAW)
Electron Beam Welding (EBW) and Laser Beam Welding (LBW)
Brazing and Soldering
Welding and Joining Brochure
Welding SmartGuide
Heat Treatment
Machining
Grinding
Descaling and Pickling
Welding SmartGuide
Welding and Fabrication Brochure
Corrosion Guide
Alloy Backgrounds
Alloy Groups
Metallurgy
Corrosive Environments
Wear Background
Abrasion
Erosion
Metal‐to‐Metal Sliding Wear
Corrosion Alloy Manual
Alloy Innovation
Alloy Development
Alloy Manufacturing
Alloy Technical Support
Specifications and Codes
Accreditations and Approvals
MSDS/Safety Data Sheets
Safety Data Sheets, English
Safety Data Sheets, Chinese
Safety Data Sheets, Czech
Safety Data Sheets, French
Safety Data Sheets, German
Safety Data Sheets, Italian
Safety Data Sheets, Japanese
Safety Data Sheets, Korean
Safety Data Sheets, Spanish
Trademarks
Technical Library
Sales and Service
Sales and Service
Sales Office and Service Center Locations
Request for Quote
Terms and Conditions of Sale
Cancellation Policy
Export Compliance Policy Letter
Due Diligence
Incoterms®
Alloys and Products Brochure
Processing Capabilities
Abrasive Saw Cutting
Bar Saw Cutting
Laser Cutting
Near-net Shaped Cut Parts
Plasma Cutting
Precision Shearing
Virtek® Laser QC®
Waterjet Cutting
Contact
Sales
Technical Support
Investor Relations
Careers
General Information
HAYNES® 625SQ® alloy
Home
/
Alloys
/
Alloy Portfolio
/
High-temperature Alloys
/
HAYNES® 625SQ® alloy
/
Physical Properties
ASP.sfctrlpresentation_openaccessdataprovider_7b98424546ba62e18cdfff0000376e70_ascx
HAYNES® 625SQ® alloy
Principal Features
Nominal Composition
Physical Properties
Tensile Properties
Heat Treatment
Specifications and Codes
Disclaimer
Alloy Brochure
Principal Features
Nominal Composition
Physical Properties
Tensile Properties
Heat Treatment
Specifications and Codes
Disclaimer
Alloy Brochure
Principal Features
Nominal Composition
Physical Properties
Tensile Properties
Heat Treatment
Specifications and Codes
Disclaimer
Alloy Brochure
Physical Properties
Physical Property
British Units
Metric Units
Density
RT
0.305lb/in
3
RT
8.44 g/cm
3
Melting Range
2350-2460°F
-
1290-1350ºC
-
Thermal Conductivity
800°F
109 Btu-in/ft
2
-hr-°F
1290-1350°C
15.3 W/m-°C
1000°F
121 Btu-in/ft
2
-hr-°F
400°C
18.3 W/m-°C
1200°F
132 Btu-in/ft
2
-hr-°F
600°C
19.8 W/m-°C
1400°F
144 Btu-in/ft
2
-hr-°F
700°C
21.5 W/m-°C
1600°F
158 Btu-in/ft
2
-hr-°F
800°C
23.4 W/m-°C
1800°F
175 Btu-in/ft
2
-hr-°F
900°C
25.6 W/m-°C
Mean Coefficient of
Thermal Expansion
70-800°F
7.7 µin/in-°F
1000°C
14.2 µm/m-°C
70-1000°F
8.0 µin/in-°F
20-500°C
14.8 µm/m-°C
70-1200°F
8.2 µin/in-°F
20-600°C
15.4 µm/m-°C
70-1400°F
8.6 µin/in-°F
20-700°C
16.1 µm/m-°C
70-1600°F
9.2 µin/in-°F
20-800°C
16.8 µm/m-°C
70-1800°F
9.6 µin/in-°F
20-900°C
17.4 µm/m-°C
Electrical Resistivity
400°F
52.8 µohm-in
20-1000°C
134.0 µohm-cm
800°F
53.5 µohm-in
200°C
135.6 µohm-cm
1000°F
54.3 µohm-in
400°C
137.9 µohm-cm
1200°F
54.3 µohm-in
600°C
137.5 µohm-cm
1400°F
53.9 µohm-in
700°C
136.5 µohm-cm
1600°F
53.5 µohm-in
800°C
135.6 µohm-cm
1800°F
53.1 µohm-in
900°C
134.8 µohm-cm
Dynamic Modulus
of Elasticity
70°F
30.2 x 10
6
psi
1000°C
208 GPa
400ºF
28.8 x 10
6
psi
20°C
199 GPa
800°F
26.7 x 10
6
psi
200°C
186 GPa
1000°F
25.6 x 10
6
psi
400°C
171 GPa
1200°F
24.3 x 10
6
psi
600°C
163 GPa
1400°F
22.8 x 10
6
psi
700°C
153 GPa
1600°F
21.2 x 10
6
psi
800°C
142 GPa
1800°F
18.7 x 10
6
psi
900°C
126 GPa