Minimal Mechanical Properties

Condition Specification Yield Strength
0.2% Offset
Ultimate Tensile
Strength
Elongation*
Annealed AMS 4943 ksi MPa ksi MPa % -
75.0 517 90.0 621 15 -
CWSR AMS 4944/4945 105.0 724 125.0 862 8 0.016 in Wall & Bellow
CWSR AMS 4944/4945 105.0 724 125.0 862 10 Above 0.016 in Wall
CWSR DAN 2700.9 95.0 655 100.0-133.0 690-920 14 1/4 in Diameter
106.0 730 126.0-149.0 870-1030 14 3/8 in Diameter
106.0 730 126.0-149.0 870-1030 16 1/2 to 1 in. Diameter

*2in (50.8 mm) gage length for AMS 4944 and AMS 4945. 1.969 in (50.0 mm) gage length for DAN 2700.9