Stress-Rupture Data

Sheet (AMS 5598)

Test Temperature Approximate Initial Stress to Produce Rupture in:
10 h 100 h 1000 h
°F °C ksi MPa ksi MPa ksi MPa
1100 600 120 825 85 585 71 490
1200 650 80 550 66 455 50 345
1300 705 61 420 45 310 29 200
1400 760 41 285 26 180 15 105
1600 815 24 165 14 97 7.4 51
1700 870 12.5 86 6.6 46 - -
1800 925 6.5 45 - - - -