Oxidation Resistance

Alloy Room-Temperature Wear Depth for Various Applied Loads
1800°F (980°C) 2000°F (1095°C) 2100°F (1150°C)
- mils µm mils µm mils µm
230® 0.7 18 1.3 33 3.4 86
X 0.9 23 2.7 69 5.8 147
Waspaloy 3.1 79 5.4 137 9.1 231
263 5.7 145 14.2 361 16.1 409
R-41 4.8 122 11.6 295 17.4 442

* Flowing air at a velocity of 7.0 ft/mm. (213.4 cm/mm.) past the samples. Samples cycled to room temperature once-a-week.
** Metal Loss + Average Internal Penetration.