Short-Time Tensile Data

Form Condition Aging Test Temperature Ultimate Tensile Strength 0.2% Offset Yield Strength Elongation
Sheet 0.063 in. thick Heat-treated for at 2150°F (1177°C), RAC °F °C Time, h °F °C ksi MPa ksi MPa %
- - - RT RT 115.1 794 45.5 314 50.7
- - - 1100 593 86.9 599 32.9 227 45.3
- - - 1300 706 69.6 480 31.6 218 30.0
- - - 1500 816 55.9 385 29.5 203 24.3
- - - 1700 927 34.0 234 25.9 179 30.0
Aged 1500 816 128 RT RT 115.4 796 49.3 340 46.8
Heat-treated at 2150°F (1177°C), then welded andtested as-welded - - - RT RT 116.1 800 - - 37.5
- - - 1200 649 71.5 493 - - 17.0
- - - 1300 704 63.5 438 - - 10.5
- - - 1500 816 52.0 359 - - 8.5
Sheet 0.045 in. thick Heat-treated at 2150°F (1177°C), then welded andtested as-welded, RAC - - - RT RT 114.4 789 44.7 308 50.0
- - - 1000 538 93.0 641 28.3 195 46.0
- - - 1100 593 93.0 641 28.9 199 50.0
- - - 1200 648 82.4 568 27.5 190 37.0
- - - 1300 704 69.9 482 28.0 193 24.0
- - - 1400 760 61.8 426 26.2 181 21.0
Aged 1000 538 10,000 RT RT 117.7 812 45.1 311 50.0
1100 593 10,000 RT RT 120.0 827 47.5 328 49.0
1200 648 10,000 RT RT 116.0 800 46.8 323 46.0
1300 704 10,000 RT RT 115.5 796 45.8 316 46.0
1400 760 10,000 RT RT 115.0 793 43.6 301 40.0
1000 538 10,000 1000 538 97.7 674 - - 46.0
1100 593 10,000 1100 593 90.5 624 - - 40.0
1200 648 10,000 1200 649 81.9 565 - - 32.0
1300 704 10,000 1300 704 76.1 525 - - 24.0
1400 760 10,000 1400 760 65.1 449 - - 20.0
Weld Metal As Welded -
- RT RT 116.1 800 - - 39.3*
-
- 1200 649 73.6 507 - - 18.1*
Aged 1200 648 500 RT RT 116.8 805 - - 38.6*
1200 648 500 1200 649 82.7 570 - - 26.5*

*Elongation in one inch
RT= Room Temperature